CHAPTER 62
1962 Guide And Dafa Book
Table 2 .... Hardness and Retained Austenite Content of Hardened and Cold Treated Tool SteeP
suit from thermal stresses caused by the localized heating ac
tion of the grinding wheel. This condition is further aggra
vated by the expansion of retained austenite transforming
thermally or by the
shock of the wheel causing
conversion to martensite with severe surface stresses. Tool steels which may show marked improvement by cold
treatment are those high in carbon nd alloy content such as high speed, high-carbon high-chrome, 1 percent carbon-5 percent chromium, and tungsten punch. A comparison of
harHngga and retained austenite content of several tool steels
after cooling to --320 F is shown in Table 2. If high speed steel is properly hardened and then tempered
at 1050 F for 2^ hr, very little retained austenite should re
main in the structure. With the usual addition of 2 or more
multiple tempering cycles at 1050 F, negligible retained austenite chniilH remain in the structure to warrant cold
treatment. However, cold treatment may serve to reduce the number of required multiple tempering cycles. When the as-
quenched retained austenite content is greater than normal,
cold treatment may be more effective than multiple tem pering. This condition may result from high quenching tem
perature, surface carburization, interrupted quenching, or the
high alloy content in special steels. Increased hardnes and cutting performance have been noted after cold treatment
and retempering when applied to stock high speed tools. This improvement might be explained by the transformation of retained austenite formed during severe grinding of the cutting edge causing rehardening of a thin surface layer.
High-carbon high-chrome (1.5 percent carbon, 12 to 14 percent chromium, 1 percent molybdenum), 1 percent car
bon, 5 percent chromium, 1 percent molybdenum die steels
respond very well to cold treatment. Multiple cycling of highcarbon high-chrome steels between --120 F and 950 F pro
duces greater stability than is possible by secondary harden
ing alone in the temper at 950 F; however the final hardness may be less than with the conventional quench and temper
process. When these steels are tempered at 400 to 500 F, an increase in b*rdnesw is noted over the conventional treatment.
Rockwell hardness inspection should never be made prior to
a 300 F stress relief since there is a hazard of incipient cracks
forming from the penetrator impression.
Wear resistance can be increased in the 1 percent carbon,
5 percent chromium steel by cooling to --150 F prior to a 400 F temper. This is particularly effective whenever the sur
face carbon content is increased by pack hardening in car burizing compound. This technique of carburizing certain tool steels to improve surface wear resistance is also used with the 0.5 percent carbon, 1-2 percent tungsten, 1 percent chrom ium punch and die steel.
HttrriMi&hlft magnet steels, such as the 1 percent carbon types with either percent chromium, 3 percent cobalt or 5 percent tungsten, tend to retain austenite in the hardening process. This non-magnetic austenite may be converted to magnetic martensite by cooling to --150 F as a continuation of the quenching cycle with a resultant increase of about 5 percent martensite.
Salvage of out-of-size tools and dies is sometimes possible by cold treatment to compensate for shrinkage in heat treatment or dimensional errors in machining of close tolerance work The expansion in volume gained by conversion of possible re tained austenite will be slightly offset by shrinkage in the subsequent tempering of the freshly formed martensite.
MECHANISM OF PRECIPITATION
HARDENING
Certain alloys may be hardened by a mechanism known ss precipitation or age hardening rather than by allotropic trans formation as in steel. This mechanism depends on the de creasing solubility in the solid state of solute atoms dissolved in the crystal lattice of a solvent 6olid solution. The heat treatment of such alloys consists of: (1) a solution heat treat ment wherein complete solution of solute atoms takes place, (2) a rapid quench, usually in water, which produces a soft supersaturated solid solution at room temperature and (3) a precipitation heat treatment which tends to permit solute atoms to aggregate and coalesce into particles of the precipita tion phase. The term precipitation is misleading in that maxi mum hardness and strength are achieved in tins operation before any visible particles of the second phase are observed in the micrestructure. It is believed that the strengthening of the crystal lattice occurs in a pre-precipitation stage of the process possibly caused by reorganization or distortion within the crystal lattice. With higher precipitating temperature, or increased time at temperature, coalescence and growth of the precipitating phase occurs to produce an overaged structure with loss in strength and hardness.
Those alloys which precipitate at normal atmospheric te* peratures and hence do not require precipitation heat treat-
Cold Treatment of Metals
663
peat for hardening, are referred to as natural age hardening alloys. They are normally furnished in the solution heat jested or annealed condition and are fabricated before natmaJ aging occurs. With some alloys the time element is such that storage after the solution treatment would permit hardering to take place prior to fabrication unless steps were taken to delay the aging phenomenon. Cold treatment has been very effective in slowing down the aging rate in such alloys.
Aluminum alloy rivets made from 2017 (17S) and 2024 (24S) aluminum will normally start to age at 32 F within 16 hr after the solution treatment. They may be stored about a Keek at 0 F and held indefinitely at --40 F without hardening firing place until after the riveting operation. A recent trend 1ms extended the use of cold treatment to solution treated PfctingB. forgings and sheet metal blanks for storage prior to cold working operations. To promote dimenmnnal stability and better machined finishes in precipitation hardenable flfrimimim and magnesium castings, a combination of cold treatment at --140 F followed by overaging 50 F above the aging temperature has been employed. This allows per manent growth to take place prior to the final dimensioning of precision parts and minimizes possible service failures caused by temperature fluctuations over the same range of temperature.
Modifications of the 17-7 type austenitic stainless steels have been developed recently to satisfy aircraft and missile operating temperatures up to 800 F. These semi&ustenitic steels are made hardenable by cold treatment at --100 F to form martensite or by a combination of cold treatment at --100 F followed by precipitation treatment in the range 750 to 1050 F.
PROCESSES INVOLVING PHYSICAL CHANGE
The preceding discussion has covered cold treating ap plications involving permanent structural change in metals. Other commercial applications of cold treatment involve revosible physical change where temperature is the controlling factor. Such processes include expansion fitting, shrink disas sembly, and a unique application employing frozen mercury for precision ranting patterns.
Expansion fitting differs from' shrink fitting in that an internal part is thermally contracted by cold treatment, inserted into a mating part, and allowed to expand to a tight fit upon returning to atmospheric temperature. Shrink fitting on the other hand involves the heating of the external part with subsequent shrinkage when assembled and allowed to cool around an inside part. A combination of both expansion and shrink fitting may be utilized when greater assembly strength is required. Shrink disassembly of bushings, sleeves and hollow inserts is possible if a suitable refrigerated coolant can be allowed to flow through the internal part.
The use of cold treatment in the assembly of parts offers a definite advantage in ease of operation with freedom from oxidation, distortion and softening caused by tempering of hardened parts when heated for shrink fitting. A disadvan tage of the process is the limited size change found possible when cooling with liquid nitrogen to --320 F compared to the thermal expansion resulting from heating through several kindred degrees.
In the Mercast process (developed by Mercast Corp.), cold treatment is employed to control the phase change between liquid and solid mercury used as replica material in place of the wax or plastic employed in the familiar lost toax or pre
cision investment casting process. Mercury is rapidly frozen in a master mold by cooling to --100 F, removed as a solid feplica of the part, and then held below --40 F during the investment proccess.
METHODS OF COLD TREATMENT
Temperatures below --150 F are seldom required for com mercial cold treatment of metala except in connection with expansion fitting. In fact, a temperature of --120 F is gen erally satisfactory except where maximum dimensional stabil ity warrants the higher cost of lower temperature intallation and operation. The various means of producing sub-atmos pheric temperatures and the temperatures obtainable are:
Salt and ice Mechanical refrigeration, tingle stage Solid CO* and methyl alcohol or acetone Solid CO* Mechanical refrigeration, multiple stage liquid air Liquid nitrogen
liquid helium
- 6F
- 50 - 100 - 109
- 150 -314
-320 - 458
Although solid CO* and alcohol or acetone mixtures require a relatively small initial investment, continued use on a pro duction basis is inconvenient and costly. Mechanical refrig eration provides the best nwinii of meeting variable produc tion demands. Such units are generally operated continuously at the desired temperature. Both liquid baths and circulated air chambers are used for cooling parts, however, the rapid heat transfer in the refrigerated liquid bath is somewhat offset by the greater tendency toward cracking. liquid nitrogen has limited commercial use except in special applications that warrant the relatively high cost.
In cold treatment sufficient time must be allowed for parts to come to uniform thermal equilibrium at the temperature of the cooling medium. The following times were required to cool machined steel cylinders, four inches in length, from an ambient temperature of 75 F down to an alcohol bath tem perature of --100 F as measured by thermocouples embedded at the middle of the bar:
Diameter, In. 1
4
Time, Min.
9 14
Id 20 26 38
It will be recalled that in those cold treating and stabilizing processes involving conversion of retained austenite to mar tensite, transformation takes place with decreasing tempera ture and is not a function of time at temperature.
REFERENCES
1 A. R. Trciano and A. B. Greninger: The martensite transfor mation (Metal Progress, VoL 50, August 1946, p. 303).
R.A. Grange and H. M. Stewart: The temperature range of martensite formation (AIMS Transactions, VoL 167, 1946, p. 467).
1 B. S. Lenient, B. L. Averbach, and M. Cohen: Dimensional stability of steel. Part IV: tool steels {American SocietyJor Metal* Transactions, VoL 41, 1949, p. 1061).
BIBLIOGRAPHY
H. C. Amtsberg: Subzero treatment of steel {Iron Age, VoL 155, January 11, 1945.p. 50).
Atlas of Isothermal Transformation Diagrams (United States_^8tee! Corp., Pittsburgh, Pa., 1951).
G. B. Berlieu: Subzero hardening cycles (Steel, January 10, 1944, p. 86).
H. E. Boyer and H. C. Miller: Subzero treatment amplifies hardening of alloy rarhuriring steels {Materials and Methods, March 1946, p. 730).
O. E. Brown: Practical approach to cold treatment of steels {Materials and Methods, December 1946, p. 1445).
S. M. Depoy: Subzero treatment to improve tool life {Metals And Alloys, \ol. 20, September 1944, p. 645).