JOHMS-MAHVILLE RESEARCH AND ENGINEERING CENTER
Tllk. STUDY OF WEAR DUST FROM BRAKE LINING ' Project 2550
Report No. **56-2506 Date December 19* 1966
SUMMARY
Brake lining veer dust was collected on a membrane filter mounted in a box which surrounded a brake rur. on an inertia dynamometer. In addition to this airborne fraction, the dust that settled to the floor of the box and that which remained within the brake was also collected. A total of 6-1/2 grama of dust was collected from 2150 stops during a total time of about 110 hours. The airborne portion was 2.7 grams. Most of the'stops were made from 35 miles per hour at 10 ft/sec2 deceleration, interspersed with stops from 50 mph (about 10 per cent).
The airborne dust was examined by light nlcroscope, electron microscope, X-rays and other means. Asbestos fiber could be detected only by the electron microscope which gave a maximum of l.fc per cent fiber by weight in the wear dust, although the lining contains 70 per cent chrysotile fiber.
This result is accounted for by the high surface temperature and severe abrasion during even the mild braking of these tests when the average temperature did not exceed 200F. Calculations show that the surface temperature at the true area of contact (1 per cent'of the apparent area) can reach 2000C or more. It is concluded that most of the fiber is converted to an amorphous mineral by intense
heat and fine grinding.
It is recommended that samples of the particulate matter in the atmosphere be collected at suitable distances from highways and the sample examined in the
electron microscope for asbestos.
k )
Contents: Summary, Introduction, Experimental Method, Results, Appendix ! culations), Appendix II (Tables 1 and 2).. Appendix III (Figures l-1*). and
Appendix IV (References).
cc: F. J. Solon, GH K. W. Smith, MB
**
Reported by:
David Sinclair Basic Physics Section
A. C. Smith (2+S F. L. Fundsack
Atts S. Spell J. Dec K. G; Koch V. C. Streib H, W, Gilbert H. F. Remde D. Sinclair Library (2)
JOHNS-klANVILtE RESEARCH AND ENGINEERING CENTER
Report No. ^ 56-2506 Page 1
awnouiiOH o r ^publication.
JM CONi; iDhi> i v \ l*. tWf tw
INTRODUCTION
laboratory measurements were made to determine what type of particulate matter and gases are given off when a brake lining ia worn during operation. The wear of the drum, usually cast iron, is necessarily included. Of special interest is the airborne dust expelled into the atmosphere from the moving brake. Previously, some observations had been made at Johns-Manville Research and Engineering Center on dust removed by hand from a laboratory brake,^ but this is the first time, to our knowledge, that any observations have been made on the airborne fraction.
A search of. the literature revealed no measurements on brake lining wear dust. although the rate of wear is sometimes given.2>3 Recently, numerous articles1*>5
have appeared calling attention to the widespread use of asbestos in materials such as brake linings, floor tile, roofing, asbestos-cement products, etc. It is usually assumed that as these materials wear, much of the asbestos fiber is dispersed into the atmosphere, thereby contributing to air pollution and creating a health hazard. This is understandable, since the asbestos content of these materials is often high, TO per cent in the brake linings used in these tests, and asbestos is commonly considered to be indestructible. However, ve know of no measurements made to test this assumption or to observe the amount of asbestos in urban atmospheres.
The present tests show that during the wear of brake linings very little asbestos fiber is dispersed into the atmosphere. Examination of the airborne dust by light microscope, electron microscope, and X-ray diffraction shoved very little of the original chiysotile fiber. Nearly all the fiber appears to have been con verted to an eoorphpua mineral by the severe abrasion and intense heat generated during brake operation. A point-count made on eight electron micrographs gave an upper limit of l.k per cent fiber in the airborne dust.
This is not surprising when one calculates the amount of energy dissipated while operating a passenger car brake. It is shown in the appendix that the heat generated
raises the temperature of the surface of contact between brake lining and drum to about 2^00C. This high temperature occurs on the surface of the lining at the regions of actual contact with the drum, much less than the apparent area of contact.6
These regions of contact are worn away during rubbing, so that the actual contact continually shifts to new regions. As a result, the wear particles of asbestos, resin, etc., are heated to a very* high temperature for a very short time. Bowden and Tabaobserved many incandescent hot spots during the rubbing of metals on glass.
EXPERIMENTAL METHOD
A wooden box, approximately a 1-1/2-ft cube with a Lucite top, was constructed to fit around a 1961 Ford brake mounted on the C inertia machine in the Friction Materials Research Section pilot plant. Figure 1 is a photograph of the box mounted on the brake. The left rear side has a conical air inlet which carries a 1-ft-square Flanders fiber glass filter oa the entrance, and tapers to a U-in.-square opening at the outlet into the box, The right front side of the box carries tvo 0 x 10-in. filter holders for Gelman membrane filters. These holders are connected through flexible hoses to a 7-1/2-hp industrial vacuum cleaner (not shown). When the vacuum cleaner was run, about 150 cfm of dust-free air was drawn through the Flanders filter, over the hreke and out through the membrane filters to collect the airborne wear dust.
The pressure drop across the membrane filters was about 15-cm Kg, measured with the
*hwi
r>n tVu* fcnx at the right connected to a netCOCk
*
JOHNS-tfAHVI11E RESEARCH
AID ENSIHEERIN& CENTER
ReportNo *
1*56-2506
Since the interior of the box was under a negative pressure of 3/b-in. HgO, it was necessary to seal the Joints end screv holes against entrance of dusty ambient air. This was done on the outside with DUX5EAL and on the inside with contact adhesive. The interior of the box and the parts of the brake and mounting vithin the box were painted white to show up any wear particles that settled out. The stationary hubs at each end of the brake drive-shaft were sealed to the ends of the box with l/l6-in. rubber sheet and rubber cement.
Figure 2 shows the auxiliary equipment used to measure the relative rate of evolution,
of wear dust during and after braking. At the left rear Is seen a Sinclair-Fhoenix
aerosol photometer connected to the side of the box through a petcock. In the left
foreground is a logarithmic amplifier connected to a Varian recorder on the right.
.
Dusty air was drawn continuously from within the box and through the photometer at a rate of about 1 cfm by means of a 1/6-hp Gast pump. Since this rate of air removal
is about 0*7 per cent of the total air flow, its reduction of the amount ox' dust
collected on the membrane filters is negligible.
Figure 3 shows the type of record obtained during stops from 35 and 50 miles per hour at 10 to 12 ft/sec^ deceleration at intervals of 2-1/2 minutes. Two of the stops were
from 50 mph as indicated and the others from 35 mph. Usually a more or less regular pattern occurred in which the dust concentration fell to near zero between each of several stops and then remained at an intermediate level for a couple of stops.
The marks numbered 2, 3, and b are calibration points for the logarithmic amplifier. They are obtained by interposing neutral optical filters of known light transmission into the photometer light beam.
'
Figure b is the resultant calibration curve which shows the approximate logarithmic relationship between chart reading and dust concentration, the latter proportional to scattered light intensity. For example, a chart reading of 50 corresponds to a dust concentration about 100 times that for a reading of 5*
Dust was collected during 2150 stops, most of it on two membrane filters The average temperature of the brake lining was kept at 175-200o? and was measured with a thermo couple set in a hole In the lining about 1/16 in. below the surface. The temperature was kept low, in order to simulate average braking, by increasing the time between stops to 3 to 4 minutes when overheating commenced. As indicated earlier, this tempera ture is far below the instantaneous surface temperature (see Appendix I )
RESULTS
Three fractions of wear dust were collected:
1. Airborne dust collected on membrane filters: 2.71 gm;
.
2. Dust removed from vithin brske. after completion of test: 3.5b ga;
f*
3 Dust collected from within box after completion of teat:' 0.2lb gm.
**
These fractions all include some cast iron worn from the drum^ about 1 gm total. The
samples were analysed for ignition loss, by light and electron microscope, X-ray
.
spectrometer, emission spectrograph, infra-red spectrograph, and Coulter particle
size analyzer. In addition, air samples were withdrawn from the box during braking and
*nnlvzed bv the Ccllob Analytical Service. Table 1 shows the results obtained.
JOHKS-MAHVILIi RESEARCH AND EN6INEERIN6 CENTER
ReportNo. ^56-2506 Page 3
Table 2 shows the composition of linings used. It Is seen that the finished lining is about 70 per cent chrysotile fiber after the water and other volatiles are driven off.
The total weight of sample collected, 6.^6 gm, is much less than the measured weight loss of the brake shots and drum: primary, U.O il gm; secondary, 7.0 il; and 2 si ga. However, the accuracy of these weights is questionable because of the heaviness of the shoes and the drum. We feel certain that negligible loss of dust occurred during the tests, so that we cannot account for the discrepancy.
1 | \
|
JM C O M ID h N 'i 1A L . A mi f o r !*/**< lim n b u tto n o r rtp u O ix a tio iL .
^
JOHNS-MANVILLE RESEARCH AND ENGINEERING CENTER
Report No. 1*56-2506 Page U
J M C O N frJO C J'*! lA i.. .\o t jc r z<r,t>Gt a u in o u u o n o r rtpuuueM UM *
APPENDIX I
Calculation of surface temperature of lining.
These tests simulate a front wheel brake of a 1961 Ford, designed to decelerate 30.5 per cent of the car mass, or 1270 pounds. At a velocity of 50 mph 73.5 ft/sec the kinetic energy of this mass is 106,000 ft-lb or 136 Btu. At a deceleration of 10 ft/sec2 this heat is generated during a stop of 7.3? seconds' duration. During the first second, the average rate of heat generation is 3l*.6 Btu per second = 8.72 x lO^ cal/sec. This heat is generated over a total lining area of 52.5 sq in. {21 x 2-1/2) rubbing against cast iron.
Bowden and Tabor^ give a method which allows a calculation of the true area of contact,
Their experiments on metals shoved that the actual area of contact is directly pro portional to the load. As the load was increased, the points of contact* flowed plastically until the area of contact was sufficient to support the load. In the case of less ductile materials such as brake linings, the points of contact would be crushed until the load-bearing area was large enough 90 that the crushing strength was no longer exceeded.
For metals, 3ovden and Tabor found that the yield pressure is three times the tensile strength. Tte make the same assumption fox brake linings. Johns-Manville Research re port U56-T-IU, received from A. J. Taylor, gives a tensile strength of 1590 psi for a lining similar to that used in these tests. The yield pressure is then pTM * 1*770 psi- 6.87 x 10S IVaq rt.
According to the definition of the yield pressure, Pg = L/a, where L is the load and a is the real area of contact. The load on the lining may be calculated by equating the torques about the axle of the simulated car.
The torque on the tires is
mdR * 1270 x 10 x 1.09/32.2
'
Here, m * mass declerated * 30.5 per cent of total mass of car 1270-lb mass, d deceleration 10 ft/sec^ * (10/32.2)g
R * rolling radius * 1.09 ft The torque on the brake lining is
^alr * 0.1* x L x 0.1*63 ^ Here, /U coefficient of friction 0.1*
L * load r - drum radius = 0.1*63 ft Equating these two torques gives the load,, L "2320-lb force.**
.
*
*- - -
*The roughness of even the smoothest brake lining (10-microinch average) Is about 2500 times molecular dimensions.
r'.*<
Mtaamom
fimttir.
We: SAKE UHUO VWR Rg?i Btftft? Of tt* W9T
Requested byi J. 0. Koch IM5&)
?^cpn/gQ
r
Susgoj^
'l , t;'
Hoar products from bm*e linings r< produced 4a a toot aeodJa* 2e tt* yrtetlra WterlAla Department* Two nine v*n *ade and tbs duit froa tU *wr product* vae collected from three locations of the teet aaeblne* The dir bone Ant via collected OelfiUA paper. gaaplo* of duet, eccaaulatad in the tna end box ware also collected.
The dust from the wear products vae examined by varloua techniques to dates!**
the nature of the products* Since ehtyectlie fiber X* the rojoj* eoartisuaot of
bra<t? 1!nines* It vae buryrising to find that the fiber vue undetected by fnj1 or
infruryd techniques. Spectrograph!e dato stove that tbe elroehtal cdUUtWKa
of cftiyrosU* fiber, that le oil!a* and aagnesu, are present proper ratio of lil.
vitn the electron microscope, however, cfcryaotUe fiber vea Identified and oeuroted
to tc i.U per cent in the air borne duet* l&ee Report 4$6*Xot*^oT}
'
iron and aognetite vrd4erlfUd by x-ray diffraction patten*. A etrtfff bend at 3-0 microre of the fSfStu epeetrue may be indicative of a pbettUe natanai,
probably e degradation product cf phenolic resin.
The mechanism by valch the eb.^sotUe fiber le aiust coepietely dsgemoroted to an aecrphous produet or products, dunce broking operations, la eot understood. HU believed that this phase of the inquiry la being investigated.
A developacnt report
vill be isaued by p. Sinclair regarding tbe mturo
of the veer products and other aspects of this work*
materials Sucnltted
Sample
Ident, F;.
Labcratory Index Fo.
Deacrimtiaa
A9*-*W A9**"3 K^k^-k
Air borne dost eboaleaUy separated
from Oelaan paper (psa l)
base m ample 1 (pa 9
that fra ira
out ctm ta
.
Methods ArolyalS
*
Fine air borne dust vea nsertd tra Oelma paper Cm l) by giaaelmg the paper la cold MB? aaS caMrJfugatioa. Jfea aelveat so* i--tied mM the M arrtliV dried
at 50C la vaeuua> saj^lee vara edAltted to sroy, >|isi nrmaplifn. ilima^mls am
infrared Uboreton** for asowrotion. Isra2 erontgaroRly acre dart ear oMdlAed
fna three location*. Only air bone dust vai collected la ra 1*