For Quality... For Color TeXOLITE Paint Products
Property owners know that color is a "must" . . . that it creates an attractive atmosphere and ex presses pride of possession. They are not satisfied with good design, structure, and comfort alone; they willingly spend money and effort for good finishes that provide beautiful colors and better appearance.
United States Gypsum long ago recognized the need for better paints for interior surfaces--par ticularly for paints readily applicable to new plas ter and wallboard. The first TEXOLITE, a powder material, was formulated to meet this need. Later paste TEXOLITE was introduced, followed by a complete line of products bearing the TEXOLITE name. The performance of these early members of the TEXOLITE family soon won recognition, and TEXOLITE acceptance has been growing ever since.
The TEXOLITE Paint line now includes fiat and semi-gloss paints for exterior and interior, ma sonry paints, texture paints, varnishes, and surface preparation materials. TEXOLITE products are lead ers in their fields because of their outstanding beauty, adaptability, ease of application, de pendability, endurance, and inherent economy.
Made always to the consistently high standards of U.S.G., TEXOLITE paints have won the acceptance of painters and decorators from Coast to Coast. The TEXOLITE slogan is the buying guide of millions:
"For Quality . . . For Color . . . Buy TEXOLITE"
1
CitiC,\C'0
TEXOUTE Accent Colon
Full rang* of deep colon. An oil ratio point for uta by itsalf or for tinting other TEXOUTE products.
Characteristics
Offan unlimited color ponibilities bacauta of the wide selection of true, brilliant colon ond their intermixes to produce blends. Clarity of vehicle allows color pigments their full brilliance. Quickly recoalable and non bleeding.
Form
Paste
Priming
Seal surfaces with TEXOUTE Sealer or other high grade pigmented oil sealer when Accent Colors are to be used in full intensity or in strong tints. See directions.
Uses
Use at a deep brilliant paint, or for tinting and blending TEXOUTE Seven Star Imperial, TEXOUTE Imperial and TEXOUTE Standard. Can be intermixed for tinting casein points, resin emulsion paints, washable calcimine, and ordinary colcimine. The Deep Col ors can be intermixed themselves In any proportion. Ideal for dis play backgrounds, show cards, scenic studios, interior decorotion.
TEXOUTE Semi-gloss White and tints. A durable semi gloss enamel for interior walls and ceilings. For use in kitchens, bathrooms and other rooms where a semi-gloss finish is desired.
Characteristics Thinned with water. Dries to touch in two hours. Large brush can be used for fast application. No ob jectionable painty odor. Recoatable. Cuts painting time and costs. Excellent washability.
Form Semi-paste
Priming Some surfaces do not require. Where necessary,TEXOUTE Sealer is suggested. See directions.
Uses Over old or new interior walls in homes, apartments, offices, stores, shops, schools, hospitals and other buildings. Can be used over wood trim if wood is sealed.
TEXOUTE Stipple Finish Provides soft attractive stipple. Available in white only.
Characteristics Ready to use as it comes in the can. Dries overnight to a soft sheen. Easy to apply--use roller, brush or sponge for stippling. Highly washable. May be tinted with colors in oil or japan colors only.
Form Ready to use.
Priming TEXOUTE sealer is recommended.
Uses Over old and new interior walls and ceilings in homes, hotel), apartment), hospitals, factories and warehouses. Can be used on any sealed surface.
/
USC InteriorCold Water Paint An economical utility paint for renewing and brightening interior surfaces. Furnished in white only.
Characteristics Starch-bound cold water paint Easily applied and readily washed off when repainting is necessary. Best results when sur faces are prepared according tc good painting practice.
Form Powder
Priming Seldom used.
Uses To brighten interiors of factorie warehouses, garages, other it dustrial structures, and farm builc Ings at low cost. Excellent fc coating pipe covering. More ecc nomical than calcimine.
O s
INTERIOR TEXTURE FINISHES, VARNISH AND CEMENT FLOOR PAINT
TEXTONE - ...
A plastic paint meeting the de
mand for a dependable, eco
nomical, easily applied texture
medium capable of satisfying
every requirement of modern
decoration. .
..
Jr.
USG Texture Paint
ixcv | :TEXOLITE Spar Varnish
A b.
papular
plastic
paint
that le ^
(' A high
quality
general
purpose
easy to use. It provides a wide . varnish for Interior ond exterior
range of texturing possibilities..$( f use. Available In high gloss or
and Is lower In price than TEX. . ft satin finish. ,
....
TONE paint,
;V ' . .
j- .
'
Characteristics
'
TEXTONE properly applied forms a texture surface of superior in solubility and hardness. Furnished in while only. Can be integrally tinted with TEXOUTE Accent Col ors or coated with another paint.
Form Powder
. Characteristics
'--Characteristics
.
t,V' '
A good working plastic paint far",
Dries to the touch In four hours;
uses similar to those secured with
i Protects and beautifies all wood
TEXTONE. Somewhat less cover*
[ finishes with a tough, durable film.
age par pound. Provides excel
Highly resistant to alkali, alcohol,
lent textures in both modern and ';{ \ scuffing and abrasion. Easy to
period styles.
, 1 i ; apply. ' r .ct m
Form Powder
i : Form
l| 1 Ready to use.
; TEXOUTE Cement Floor
'i Point
^
; A breather type paint for cement
' floors. Available in six attractive
I colors. r . , i -i- ..
'
' .
.
..
Characteristics
' - ' Dries to a beautiful, washable : ` flat finish. Thins with water. Dries
overnight. Applied with large brush. Excellent base for wax coatings. For Interior or semi . protected interior surfaces.
A
Form
Paste
.
Priming
Prime surface as needed.
Uses
For producing light, soft, modern textures as well as Ihe more rug ged period designs over any dry, solid, clean interior surface. For decorating work over new ploster, gypsum wallboards, and in sulating wallboards. Especially useful in reflnishing cracked plas ter surfaces; for producing stone effects, antique effects and stencil work.
Priming Prime surface as needed.
Usos For Interesting textures over dry, clean, solid surfaces such as new plaster, gypsum wallboards. In sulating wallboord surfaces, etc. Alto on old cracked plaster sur faces.
. , Priming
' | May be used as a sealer when : : thinned with a maximum of one
pint turpentine or mineral spirit! per gallon. On open-grain woods, such at oak, use wood-filler.
t
; Use*
1 ! For floors, woodwork, furniture, porches, doors, decks, spars, etc.
Priming Prime surfaces with TEXOUTE Primer.
Uses For basements--cement floors-- porches--steps.
O 0 o
TEXOLITE Spoiling Putty
Used for preparatory treatment of surfaces before painting or decorating to build up or fill im perfections, and to produce a smooth, even surface.
Characteristics
' -v
Exceptionally fine grind. Grit-
free. Adaptable to knife or brush
application. Can be sanded. Ad
heres to any properly cleaned,
solid surface. Hardens in a few
hours, forming a tough durable
surface. ...
.
Form Powder
-' ' '.
Priming
Takes any standard aiming ma larial.
Uses
Filling small cracks, scars, slight imperfections in plaster, nicks, cracks, knotholes, or nail holes in wood trim. Spotting nail holes, cracks or joints in wallboards. To All voids or imperfections in con crete, cracks in tile or mosaic, for treating canvas and wall fabrics. For household repairs on mould ings, furniture, toys, etc. For mak ing Swedish Putty,
-RED TOP Patching Plostbr
A plaster scientifically compound
ed for patching cracks In -walls
and ceilings easily and efficiently
. at minor expense.
fasnt
v .. .r. . -v
'' Characteristics
^
Very white. No harmful shrink age. Contains no lime. Sets In 1 to 1 Vi hours. Uniform set end quality. Smooth and plastic be- ' cause of special Ingredients. '
' Form Powder
'
.
Priming
Takes ony standard priming ma terial.
\*`-
RED TOP
Painter's
Plaster :1^'1
. ,t-
> PERF-A-TAPE Joint System
if, . .
t
j.-Plaster of Paris for generafv*^, ^ Designed to conceal and rein- j
i. painters' use. Made from spe- .^ force craduil Package contains
dally selected white gypsum. -,'vi^-i 4 all needed materials,,,^'. .
^Charadrltic*
...
'-***- ...
^
"'Mixes readily, works easily, but'',jj
{' requires more careful handling,-^
thon RED TOP Patching Plaster.
f> \ Provides hard, dense and strong ^
""surfaces. Setting time opproxi--^
. mately 30 minutes.
' e - '
*[ -" xvs*K.' S'" i
^'Characteristics
.Provides - complete concealment
:.and adequate reinforcement.
{^.Combines sturdy fiber reinforce-
Ament and plastic cement. ,
M
H " ;.<i; v...Vc y
Form Powder
-f .
..-.A;;'
Form . .':'. .. . Powder and Reinforcement.
Priming
--
Takes any standard priming ma terial.
Priming None.
Uses
For patching cracks and larger breaks in plaster walls and in terior concrete surfaces. Can be decorated with any decorating material.
Uses
Recommended for patching cracks and breaks in plaster and wher ever a painter's plaster is used.
Uses
.
Used In both new and old con
struction. Developed for treating j joints in wallboard. Used to rein- s\: force cracks in all kinds of wall surfacing! especially in corners^ or at angles before redecorating,
J. s... - - - A.<, y.
<r>
*0
o
$
'-efJ
CO
o O'
Veneer Finishes
Veneer finishes oiler the opportunity to trim days from interior finishing schedules and provide strong, highly abrasionresistant surfaces These products are designed lor one- or Iwo coal work over gypsum bases or directly to concrete block or propeily prepared monolithic concrete Formulated (or hand or machine application (Diamond Finish--hand only), they pro vide a thm. lightweight veneer that sets rapidly
advantages
Rugged, Abuse-resistant Surfaces--High-slrengih Imperial Finishes (3,000 psi compressive strength) provide hard, durable interiors that require minimum maintenance.
Quicker Completion/Faster Occupancy--Veneer finishes apply rapidly, set fast, dry quickly to savp days in finishing interior walls and ceilings. Diamond Interior Finish can be decorated in 24 hrs with breather-type paint or left undecorated i( desired.
Competitive Costs--Veneer finishes are easily applied and cover more area per ton than conventional plasters Joints and inlenor angles are pre-set with the same veneer finish that goes on the walls and ceilings, eliminating need for joint compound and resultant drying tune
Easily Decorated--Veneers are readily finished in smoothtrowel, float or texture surfaces. The hard, smooth surface is decorated easily and economically with paint, fabric, wallpaper or texture
Versatile--A wide choice of assemblies is available to meet design requirements. Fire and sound-rated systems for wood or steel framing, hard and abuse-resistant surfaces for high-traffic areas, electrically heated ceilings.
products available
IMPERIAL Basecoal--For use as a basecoat in two-coat veneer application finished with proper lime or gypsum finishes Can be applied to either Imperial Gypsum Base, directly to concrete block, or over a bonding agent on monolithic concrete Formu lated as the basecoal for high-strength Imperial Finish, gauged lime putty. Diamond Interior Finish. STRUCTO-GAUGE-Iimesinoolh trowel, or Keenes-lime-sand float finishes Available in hand- and machine-application formulations. Complies with ASTM C587 and Federal Specification SS-P-00402B, Type VI. Available in 80-lb. bags
IMPERIAL Finish Plaster--For single-coat application com posed ol scratch coal and immediate doubling back (except in suspended or furred ceilings), directly over special1 Imperial Gypsum Base, glass-fiber tape or Perf-A-Tape and Durabond Compound or over Imperial Basecoat Plaster in two-coat sys tem Available for hand application--provides a smooth-trowel or float or spray-texture finish ready for decoration Complies with ASTM C587 and Federal Specification SS-P-00402B, Type VI. Available in 80-lb. bags.
veneer finishes 73
GP038 2175
When abraded 2.500 cycles with weighted wire brush (273 psi/ in laboratory test.
IMPERIAL Veneer finish showed virtually no penetration-
proof of outstanding abrasion resistance
IMPERIAL Finishes--Coverage
ft'/ton
"'/tort (mfll/kj1'1
product
imperial
Basecoal
gypsum
3250-4250
mjidnry
2700-3600
gypftitfn b)M
335-435
iKMry
275-370
IMPERIAL (i-coat) Finish
3500-4000
IMPERIAL (2-coat) Finish
3200-3600
'"Coverage rounded to nearesl 5m'
not recommended
not applicable
360-410 330-370
not recommended
not applicable
DIAMOND Interior Finish--A white finish formulated lor hand application directly over Imperial Gypsum Base or in a two-coat system over Imperial Basecoat Plaster. Applied to a nom '/i*~ thickness, this finish is unaggregated lor a smooth or skipIrowel finish; may be job-aggregated lor float or other textures. Fast-applying, can be decorated in 24 hours with breather-type paint or left undecoraled Not recommended over Portland cement basecoal Complies with ASTM C587 and Federal Speci fication SS-P-00402B, Type VI. Available in 50-lb bags
Diamono Interior Finish should be applied only to Imperial
i'
08 drywall & veneerapplication
.dnesive Lamination (Double Layer)--Produces the finest in;nor surfaces. Adhesive attachment of face layer to base layer i double-layer construction and of single-layer board to inrior masonry walls usually requires only supplemental menamcal fastening until adhesive attains full bond Reduces or immates nails or screws reouired. saves finishing labor and mimizes fastener pops and pint ridging. Durabond 210 nnt Compound is required lor adhesive lamination with fireted assemblies.
erpendicular vs. Parallel Application
/psum board may be applied perpendicular (long edges of >ard at right angles to the framing members) or parallel (long ges parallel to framing). Fire-rated partitions may require rallel application (see Chapter 3 for specific systems). rpendicular application generally is preferred because it ers the following advantages Reduces the lineal footage of joints to be treated up to 25%. Strongest dimension of board runs across framing members. 3ridges irregularities in alignment- and spacing of frame mbers. Setter bracing strength--each board ties more frame mems together than does parallel application. lorizontal joints on wall are at a convenient height for thing.
//
irting at ceiling line, horizontal board is screw-attached I Parallel application (right) is used in special situations. all application, if ceiling height is 8'1" or less, perpendicu plication results in fewer joints, easier handling and less g. If ceiling height is greater than 8T' or wall is 4 ft. wide or parallel application is more practical. For ceiling applicause whichever methods results in fewer joints, or is ed by frame spacing limitations.
Doara application 109
For double-layer ceiling application, apply base-layer boards perpendicular to Irame members, apply face layer parallel to framing with |omts offset. On wall, apply base layer parallel with long edqes centered on framing, apply face layer perpen dicular Exception when using Textone Vinyl-Faced Panels tor lace layer, apply base-layer boards at right angles to studs
drywall and veneer base application
General Recommendations for gypsum panels and gypsum bases applied to wood and steel framing:
1. Apply ceiling boards first. `
2. Cut boards so that they slip easily into place
3. Butt all joints loosely. Never force panels into position.
4. Place tapered or wrapped edges next to one another
5. Never place a butt end or a cut edge next to a tapered or rounded edge Wherever possible, apply boards perpendicular to framing and m lengths that wilt span ceilings and walls without creating end (butt) joints. If butt joints do occur, stagger and locate them as far from the center of walls and ceilings as possible.
6. Support all ends and edges of gypsum board on framing, except long edges at right angles to framing tor face layer of some double-layer applications (exceptions are specified in Chapter 3 uystem descriptions), and where end joints are to be floated between frame members and back-blocked (BackBlocking is covered later in this chapter).
7. If metal trim is to be installed around edges, doors, or windows, determine if trim is to be installed before panel application. Reter to Chapter 1 for description of products, and Chapter 2 for installation.
8. Do not anchor panel surfaces across the flat gram of wide dimensional lumber such as floor joists and headers. Float panels over these members or provide a control joint to com pensate for wood shrinkage
9. To insure level surfaces at joints, arrange board application so that the leading edge of each board is attached to the open or unsupported edge of a steel stud flange To do this, all studs must be placed so that their flanges point in the same direction. Board application is then planned to advance in the direction opposite to flange direction. When this simple procedure is followed, attachment of each board holds the stud flange at the joint in a rigid position for attachment of the following board. If the leading edge of gypsum board is attached to the web edge of a flange, the open edge of the flange can deflect under the pressure ol attachment of the following gypsum board. Friction between the tightly abutted board edges can then cause them to
JMJ drywall 4 veneer/application
bind, preventing return o( the second board to the surface plane of the first. A stepped or uneven joint surface results. This recommended application procedure is absolutely essen tial for good results in steel-framed veneer and drywall assem blies. (See drawings following for correct methods.)
r
- Election, of gypsun board installation
Tits':
) i
VV r
deflection point--Mh panel*
M
Correct application
board application in
board by scoring the tace paper, snapping the board core and then culling Ihe back paper. The common tool used to score and cut gypsum board is a utility knile with replaceable blade. Regardless ol the type knite used, its blade should be kept sharp SO that Score will be made through paper without tearing or rolling it up. and into Ihe gypsum core
For cuts across the board width, a straightedge is recommend ed. An aluminum 4-ft. drywall T-square, ruled on bolh edges, facilitates clean, straight cuts. Tor cuts along the long length ol the board, use a steel tape with an adjustable edge guide and a tip that accepts the utility knile blade. With this tape the edge guide is set tor ihe desired width and placed against the board edge The knife blade is then inserted into the slotted tape tip. and by moving both hands together the toot is drawn down the lull length ol the board to make a smooth and accurate cut.
GP038 ?L?7
ditection ol gypsun board installation
y.'A ' i~r deflection point--1 / ^--deflection point--
huTllu.
-edges bind Incorrect application
s ,/ 7 >?
Measurements--All measurements must be accurate. Make two measurements as a check. This procedure will usually warn ol partitions or door openings that are out ol plumb or out of square Then, framing corrections can be made before the board is hung. A 12- to 25-11. steel power tape is recommended. Tools lor measuring and cutting are shown in Chapter 8.
Cutting--Make straight-line cuts across full width or length o<
left to right, gypsum board is cut by scoring with utility knife against drywall T-square, then snapping toward back (top), (idling back paper with same knife and separating sections (Mow)--quick method to obtain clean edges and precise tit
r
i drywall & veneer, application
int treatment application-- ;neer construction
jnventional Method
Normal Drying Conditions--Align Imperial Type P (prese-sensitive) Tape over joint and press into place over entire gth. Eliminate wrinkles and assure maximum adhesive bond pressing entire length of tape with steel finishing knife or vei. Press tape into corners with corner tool; do not overlap.
Simplified, wrinkle-tree attachment ot self-stick Type P IPERIAL Tape speeds joint reinforcing, boosts production.
attach Imperial Type S Tape with spring-driven hand stapler ig J/" staples. Use two staples at each end of tape; staple ainder at staggered 24" intervals. At wall-ceiling angles, >le every 18" to 24" along ceiling edge only. For wall-to-wall rior angles, staple every 18" to 24" on one edge only, working i top to bottom. Position tape to bridge the joint at all rior corners without overlapping.
Lower-cost Type S IMPERIAL Tape is iidly stapled over Hat joints at staggered ervals. High-strength tlass libers and open eave of tape provide r excellent keying ot veneer finish during
embedding.
ed tape and fill beads with coat of Interior Finish being 1. and allow to set--but not dry--prior to finish application. Kly underfill in the Dead by screedmg along the bead with i of irowel after setting the bead. (Best results are obtained
i
I
t t i
<
t
veneer joint treatment 149
by planning the finishing to permit continuous application from angle to angle.)
Alternate Method
For Rapid Drying Conditions--When building temperaturehumidity conditions fall in the "rapid drying" area of the graph (below), use Perf-A-Tape Joint Reinforcing Tape embedded with Durabono Joint Compound.
Mix the compound in a clean 5-gal. container (plastic is pre ferred for Durabono). Use a commercial potato masher or a '!i" heavy-duty 200- to 300-rpm electric drill with a cage-type paddle. Drill speed must not exceed 400 rpm. Use the amount of water shown on the bag and always sift the powder into the water to insure complete wetting-. Stir vigorously for 3 min.; if lumps remain, allow the mix to soak for 15 to 20 mm., then re-stir until smooth. Note: Do not contaminate compound with other materials, dirty water or previous batches. Do not retemper batches
Butter joints with compound using a trowel or steel finishing knife to force compound into the joints. Center Perf-A-Tape over joint and press it into the fresh compound with trowel held at a 45 angle. Draw trowel along joint with sufficient pressure to remove excess compound.
After tape is embedded, apply a skim coat of joint compound to reduce possibility of edge wrinkling or curling. Allow skim coat to harden, then apply a fill coat, feathering 3" to 4" beyond edges ot tape. Allow to harden before finishing. Plaster pre-fill is not required over Durabono Compound.
Note: Under the following conditions Durabono Compound and Perf-A-Tape Reinforcement (alternate method) must be used: (1) where 2-coat finish is applied over '/j' base on 24" o.c. framing, (2) where 1-coat Diamono Interior Finish or Imperial Finish is applied over 5/" base on 24" o.c. framing.
veneer finish application
Veneer finishes can be used in one- or two-coat applications and can be given smooth or textured surfaces. Each method has its particular advantage.
Two-Coat Veneer Finish--Compared to many other finishes. two-coat veneer provides a more durable, abrasion-resistant surface and can be finished to a truer plane than one-coat applications. These finishes can be used with steel or wood framing wherever the ultimate in appearance is desired Ready for next-day decorating, assemblies with these monolithic gypsum surfaces offer excellent fire and sound ratings.
One-Coat Veneer Finish--Provides a hard monolithic surface at low cost. Complete application--from bare studs to decorated walls and ceilings--takes no more than 48 to 72 hr. Assemblies with one-coat veneer application meet fire and sound requirements. and shorten construction schedules for added profit.
Ct
ii i l
:
>
; , 1 i i . ' , j i ;
GP038 2178
150 diyvv.il! A veneer /application
Job Environment
Maintain building temperature in minimum comfortable working range, about 55 to 60F ; keep air circulation at minimum level prior to. during and following application until (imsh is dry.
Drying Conditions--Veneer Finishes
II possible, maintain building temperature-humidity combina tion in the "normal drying" area of the graph. When dry conditions exist, relative humidity olten can be increased by wetting down the floor periodically During these periods, make every ellort to reduce air movement by closing windows and deltecting heater blower and duel output away from the sur faces being plastered It building temperature-humidity combination is in the "rapid drying" area of the graph, special joint treatment measures must be taken These include the use ol Durabond 210 Joint Com pound and Perf-A-Tape Reinforcing Tape.
Grounds
Correct thickness ot veneer finish is one ol the most important factors in obtaining good results. To insure proper thickness, all
veneer finishes 151
corner beads, trim and expansion joints must be ol the recom mended type and be property set Accessories must provide grounds lor the following minimum plaster thicknesses 1. Over veneer gypsum base, one coat ...... '/i* in (1 6 mm)
2. Over veneer gypsum base, two coats.......... 3/u in (2.4 mm)
Mixing and Proportioning
All veneer finishes require the addition ol water on the |ob. Water should be clean, fresh, suitable lor human consumption, and free from mineral and organic substances that affect the plaster set. Water used lor rinsing or cleaning is not suitable lor mixing because it accelerates the plaster set. Mechanical mixing is mandatory for veneer finishes and Red Top Radiant Heat Plaster. Mix no more material than can be applied before set begins Since veneer finishes set more rapidly than most conventional plasters, always consult bag directions lor specific setting times. Veneer plasters and finishes will produce mortar ol maximum performance and workability when the correct equipment is used and mixing directions carefully followed. Proper mixing is one ol the mosl important, factors in producing mortar of maximum workability. Use a cage-type mixer paddle driven by heavy-duty ' V electric drill with a rating ol 900 to 1.000 rpm. Do not use propeller-type paddle or conventional mortar mixer. (For details of the cagetype mixing paddle and available electrical drills, see U S.G. technical data sheet P-502.)
Cage-type mixing paddle is designed to draw material into and through paddle blades to disperse and blend ingredients by shear action rather than folding action ot conventional mixers.
Mix plaster in 12 to 15-gal smooth-sided container strong enough to withstand impacts that could cause gouging Do not use brittle containers lor mixing Correct mixing--rapid and with high shear action--is essential lor proper dispersion of plaster ingredients Slow mixing can reduce plasticity of material. Overmixing can shorten working time. Operated at correct speed, the cage-type type paddle mixes thoroughly without introducing excess air into the mix
152 drywall & veneer application
DIAMOND interior finish
Water requirement tor Diamond Interior Finish is 12 to 15 at of clean water per 50-lb. bag. Place all but 1 or 2 gt. ot water into mixing container; then with mixer operating, slowly add one bac of material If desired, up to 50 lb. clean silica sand may be added per 50-lb. bag of finish. When material is wetted, ado more water (i to 2 qt.) to obtain desired consistency Mix lor minimum of two minutes, but no longer man live minutes.
IMPERIAL plasters
Water requirements for Imperial Veneer Plasters.
Imperial Basecoat--8 to 10 qt./80 lb. bag
Imperial Finish--11 to 13 qt./80 lb. bag.
Place water m a 12-*to 15-gal. smooth-sided container Start mixer, slowly add plaster and mix at least 2 min. to disperse lumps completely. Do not mix more than 5 min.
For sand float finish, add up to 20 lb. clean silica sand per 80-lb bag of Imperial Plaster to achieve desired texture. The use ol more than 20 lb. of sand per bag will decrease hardness of sur face. (Apply plaster in normal manner but omit final troweling Alter surface has become firm, float to desired texture, using sponge, carpet or other float. Use water sparingly.)
RED TOP radiant heat plaster
Red Top Radiant Heat Basecoat--Place approx. 11 to 13 qt. of
clean water in a 12- to 15-gal. smooth-sided container, and with mixer operating slowly add 80-lb. bag o! plaster. Mix lor a minimum of two minutes, but not longer than five minutes to disperse all lumps completely.
Keep mixing equipment and tools clean. Do not mix more than can be applied in 30 minutes. Do not relemper.
Red Top Radiant Heat Finish--Place approx. 12 to 15 qt. of clean
water in a 12- to 15-gal. smooth-sided container, and with mixer
operating, slowly add one bag of plaster. Mix tor a minimum ol
two minutes, but not longer than five minutes to disperse all
lumps completely.
*
Keep mixing equipment and tools clean. Do not mix more than can be applied m 30 minutes. Do not retemper
Application
Maintain temperature m all work areas at mm. 55 to 60F Keep air circulation at minimum level during and alter application until finish is dry.
DIAMOND interior finish
All finish materials and finish surfaces must be protected from conlact with Diamond Interior Finish. This includes glass, ce-
GPO38 2180
DURABOND 90 Joint Compound
Durabond 90 Compound is equally suilable (or filling form otlsets and voids lelt in interior concrete. As with COVER Coat, Durabond Compound should not be applied over moist surfac es or surfaces subiect to moisture, or any abnormal condition.
application
1. Grind off all projections on concrete surfaces.
2. Remove all dirt, grease and lorm oil from concrete surface.
3. Mix compound according to bag directions.
4. Apply to fill all otlsets and voids in concrete.
5. After Durabond has hardened (not necessarily dry), apply a skim coat of USG Ready-Mixed All Purpose or Topping Com pound over entire surface.
6. When dry. sand surface as necessary.
7. Paint or decorate surface as desired.
special applications and constructions
Integral Plaster Chalkboards
Plaster chalkboards otfer maximum freedom in design. There is no limiting sheet size as is the case with fabricated boards; therefore, entire walls can be utilized as chalkboards. Mainte nance is accomplished as easily as with conventional fabricated chalkboards. (Requirements for control joints in chalkboard surfaces are the s; ne as for other gypsum surfaces.)
chalkboard with steel stud*IMPERIAL partitions
Follow directions lor system construction. Chapter 3. Locate floor and ceiling runners and position studs 16" o.c. Attach '/>' Imperial Gypsum Base using 1" USG Type S Screws spaced 16" o.c. When chalkboard area does not extend from floor to ceiling, use 701-A or 801-A Metal Trim to frame the Vi" Imperial Base face layers that will be used as chalkboard. (All chalkboard surfaces must have two layers of IMPERIAL Gypsum Base.) Miter corners ol the metal trim to form a neat joint. Attach chalkboard using 1Vi" Type S Screws, driven through Imperial base layer into the studs. Veneer Application; use one- or two^coat plaster lor chalkboard surface With one-coat work, apply Imperial Fi'nish Plaster to Vi" to J/3j" thickness. Cover entire area with a tight, thin coat, then double back to full thickness After surface has become lirm, final-trowel to a smooth surface, using water sparingly. For two-coat application, apply Imperial Basecoat Plaster to Vi" to '/it" thickness as described for single-coat application.
Allow basecoat to set and dry. then apply Imperial Finish Plaster, Diamond Interior Finish or SmuCTO-GAUGE-lime smooth-trowel finish plaster Leave surface very hard and pol ished
Paint chalkboard, when dry, with one coat primer-sealer and two coats chalkboard paint.
Install chalktrough with USG 1J/i" Type S Screws, driven through the two layers of Imperial Gypsum Base and into the steel studs.
Vapor Barriers
Foil-Back Sheetrocx Panels when applied with their toil sur face next to exterior framing provide an effective vapor barrier that helps prevent interior moisture from penetrating into stud and joist spaces.
This system helps to maintain comfortable room humidity year 'round. Generally, during cold weather, a 10% increase in indoor relative humidity allows a 1*F. lower temperature with no de* crease in comfort.
In addition, thermal insulating value is obtained when the foil backing faces an air space of min '//.
Foil backing is not recommended in air-conditioned buildings located in the hot. humid climates of southern Atlantic and Gulf Coast areas, where a vapor barrier is required on the exterior side of walls and ceilings.
Perimeter Isolation
The perimeter of non-load bearing gypsum board surfaces Should be isolated from all structural members, except the floor. Isolation is important to reduce potential cracking in partitions, ceilings, wall, column, and beam furring. Generally, methods for
GP038 2131
Perimeter relief at columns reduces possibility of cracking.
2. Check accuracy ot alignment and position of Iraming accord ing to plans and details
3. See lliat partitions are straight and true; ceilings level
4. Measure spacing ol studs and toists Spacing should not exceed maximum allowable lor the system.
5. Look lor protrusions ot blocking, bridging, or piping, and twisted studs and joists that would create an uneven surface. Correct situation before board attachment
6. Make sure there are appropriate blocking and support for fixtures and boards.
7. See that window and door frames, electrical and plumbing fixtures are set for the board thickness used.
8. Check for proper position and attachment ol resilient and furring channels.
9. Review all wood Iraming lor compliance with minimum Iraming requirements outlined in Chapter 2.
10. Examine steel studs at corners, intersections, terminals, shelf-walls, door and borrowed light frames for positive attach ment to floor and ceiling runners.
11. Inspect spliced steel components for proper assembly.
12. See that steel stud t inges all face the same direction.
13. See that preset door and borrowed light frames are securely altached to stud and runner rough framing at all anchor clips.
14. Make sure that door and borrowed light frames will be spot-grouted, as required.
suspended grillage
1. Measure spacing of hangers, channels and studs to see that they are within allowable limits
2. Check ends of main runner and furring channels. They should not be let into or supported by abutting walls, and should extend to within 6" of the wall to support a furring channel.
3. Make sure furring channel clips are alfernated apd that luiring channel splices are properly made.
4. See that mechanical equipment is independently supported and does not depend upon the grillage for support
5. Inspect construction around light fixtures and openings to see that recommended reinforced channel support is provided.
job inspection 34
drywall and veneer installation Base layer
1. Verily that material being used complies with specifications and (ire or sound-tested construction.
2. Make sure lhat proper perpendicular or parallel application of board is being used, and that |omts are staggered
3. Check for cracked and damaged-edge panels, and see that they are not used.
4. See that the recommended fasteners are being used and spaced properly
5. Check for proper use of acoustical sealant
6. Inspect installation to make sure insulating or sound attenua tion blankets are properly attached and fitted
7. Be certain vapor barrier is installed as required.
8. Review appropriate system construction and application, and inspect for compliance with laminating recommendations and other construction procedures On fire-rated assemblies, be sure that Durabond Joint Compound is used lor lamination
9. See that required control |oints are properly located and installed.
Face Layer__________ ______ _____ 1. Verify material compliance.
2. Look for high-qualily workmanship Cracked or damagededge boards should not be used Board surfaces should be tree of defects; joints correctly butted and staggered.
3. Check tor proper application method--perpendicular or par allel.
4. Examine fasteners for compliance with specifications, proper spacing and application.
5. Review adhesive application method and see lhat recommen dations and specifications are being followed
6. Inspect trim, corner beads and related components for align ment, grounds, secure attachment and proper installation
7. Make sure that acoustical sealant is applied around electrical outlets and other penetrations and completely seals the void.
Fasteners 1. Make sure recommended or specified fasteners are used
2. See that fasteners are applied starling in center o( board and working to ends and edges.
3. Observe whether board is held tightly against framing Test lor loose board by pushing adjacent to the lastener See that face paper is not broken when fastener is driven It necessary, a second lastener should be driven within 1 /*" of the faulty one.
4. Examine lastener positions. Fasteners should be at least '/* in from edges and ends.
5. Make sure that lastener heads in veneer assemblies are flush with the gypsum base surface, not dimpled.
_______________________ Adhesives____________ ____
1- See that adhesive is applied to clean, dry surfaces only.
4
2. Make sure that board is erected within allowable time limit after adhesive is applied so proper bond can be obtained
3. Measure size of bead and spacing, and see that a sufficient quantity is applied.
4. Observe impacting blows (or proper spacing and positioning.
5. Make sure temporary fastening and shoring holds panel tightly in place.
6. Review appropriate adhesive application methods (Chapter 2) and inspect tor compliance.* 1 2 3 4 5
___ ______________ Joint Treatment--Drywall
1. Make sure panel surface is ready for joint treatment. Fastener heads should be properly seated below panel surface. Protru sions should be sanded below level of surface. Joints between panels should be filled with joint compound before taping.
2. See that recommended mixing directions are followed (see Chapter 2). Only clean water and mixing equipment should be used. Durabond Joint Compounds cannot be held over or retempered.
3. Inspect joints and corners to see that tape is properly embed ded and covered promptly with a thin coat ol joint compound. Only compounds suitable lor embedding should be used. Heavy fills should be avoided.
4. Make sure that compound is used at its heaviest workable consistency and not overthinned with water.
5. Check to see that joint compound is allowed to dry thorough ly between coats (see Drying Time Guide, Chapter 2). Exception: Durabond Joint Compounds need only have hardened prior to the fill coat application.
/on inspection J4J
6. Inspect second and thud coals over joints lor smoothness and proper edge leathering
7. See that lastener heads and metal trim are completely cov ered.
8. Make sure that all finished joinls are smooth and dry before decoration. Sand smooth il necessary.
____ __ Joint Treatmentjnd Finish--Veneer
t. See that corner bead is properly attached and aligned at all outside corners.
2. See that control joints are properly installed where required.
3. See that proper joint reinforcement is used--Imperial Tape for normal conditions. Perf-A-Tape plus Durabond Joint Com pound for abnormal job or weather conditions
4. See that Imperial Tape is not overlapped at intersections
5. Be sure that all taped Imperial Base joints are preset before finish application begins.
conventional plaster installation
__ __________
_ Plaster Base
1. See that material being used complies with specifications and fire or sound-tested construction.
2. Review appropriate system construction and application, and inspect tor proper installation practices.
3. Check for proper application ol base perpendicular to fram ing members, and see that joints are staggered.
4. Check (or cracked and damaged edges of plaster base. These should not be used.
5. See that the recommended fasteners or clips are being used and spaced properly.
6. Check lor proper use of acoustical sealant.
7. Inspect installation to make sure that insulating blankets are properly attached and fitted.
8. Be sure that adequate supports are in place for fixture and cabinet application.
_______________ Grounds JorJ'lasterlng _
The thickness ol basecoat plaster is one ol the most important elements ol a good plaster job. To insure proper thickness ol
_
gmunds should be pioperly set and lollowed The lollowing ponds should be checked:
1. All openings should have specified plaster grounds applied as directed
2. it plaster screeds are used, the dots or continuous strips of plaster must be applied to the ground thickness to permit proper plumbing and leveling.
3. Grounds should be set for recommended min. thickness for particular plaster base being used (see Chapter 5).
Job Condit_ions for Plastering
This phase of inspection is also important. An accurate check ol the lollowing points should be made periodically:
1. At no time should plastering be permitted without proper heating and ventilation. Circulatiop of air is necessary to carry oft excess moisture in the plaster, and a uniform temperature in a comfortable working range helps to avoid structural movement due to temperature differential.
To prevent dryouts," precautions must be taken against rapid drying belore plaster set has occurred. Check temperature during damp, cold weather where artificial heat is provided. During hot, dry summer weather, cover window and door openings to prevent rapid drying due to uneven air circulation.
2. Inspect plaster surfaces during drying. Setting of basecoat plaster is indicated by hardening of plaster and darkening of surface as set takes place. Plaster that has set but not yet thoroughly dried will be darker in color than the unset portion, which accounts for the mottled effect as the plaster sets.1 2 3 4
____________ Plaster Application ______
Alter determining what materials are to be used on the job. refer to correct mixing and application procedures described in Chapter 5. The visible success of the job is at stake with the finish plaster coat, and required measures should be taken to finish correctly:
1. Check plaster type and mixing operation.
2. See that proper plaster thickness is maintained.
3. Consult architect's specifications to see that proper surface finish method is being used.
4. Check temperature of building for proper finish plaster dry ing conditions.
Cleanup
For a complete job. cleanup is the final stage. All scaffolding,
, 1
' i [
,!
i i I J , , ti i I j ,
empty containers and excess materials should be removed horn the |ob site Floors should be swept and the building and site left in good condition for decoration and finishing
I
GP038 2184
problems: their cause, remedy and prevention
The first part of this chapter deals with problems associated with gypsum construction, many of which are beyond the control ot contractors working from construction documents.
Other problems, resulting from improper job conditions and application practices, are the direct responsibility ol the con tractor and can be controlled by him. These are discussed fully in the following section, together with corrective action to remedy the problem and prevent future recurrence.
Drywall Construction
Almost invariably, unsatisfactory results show up first in the areas over joints or fastener heads Improper application of either the board or joint treatment may be at fault, but other conditions existing on the job can be equally responsible for reducing the quality of the finished gypsum board surface
To help determine the exact problem cause, the physical appear ance of each defect is described here along with a discussion of the factors causing unsatisfactory results. The checklist following contains possible causes for the irregularity and serves as an index to the numerically listed problems, causes, remedies and preventions. By checking each numerical item listed for the defect, the exact problem cause can be determined and appropriate correction action taken.
description of defect
Fastener Imperfections--A common defect which lakes on many forms. May appear as darkening, localized cracking or a depression over fastener heads, pop or protrusion of the fasten er or the surface area immediately surrounding the fastener. Usually caused by improper framing or application of fasteners.
Joint Defects--Generally occur in a straight-line pattern and appear as ridges, depressions or blisters at the joints, or darkening over the joints or in adjacent panel areas Imperfec tions may be result ol incorrect framing or joint treatment, or climatic conditions if remedial action has not been taken.
Loose Panels--Board does not have tight contact with framing, rattles when impacted or moves when pressure is applied to the surface. Caused by improper application of panels, framing out of alignment or improper fastening.
Joint Cracking--Appears either directly over the long edge or butt ends of boards, or may appear along the edge ol taped joints. Olten caused by structural movement and/or hygrometric
and thermal expansion and contraction, or by excessively last drying ol joint compounds
Field Cracking--Usually appears as diagonal crack originating Irom a corner ol a partition or intersection with structural elements Also seen directly over a structural element in center of a partition May originate from corners of doors, light fixtures and other weak areas in the surface created by penetration. Caused by structural movement described earlier in this chap ter Also see Perimeter Isolation and Framing--Door and Win
dow in Chapter 2 lor use of control joints to minimize cracking.
Angle Cracking--Appears directly in the apex of wall-ceiling or
interior angles where partitions intersect Also can appear as cracking at edge of paper reinforcing tape near surface inter
sections. Can be caused by structural movement or improper application of joint compound in corner angle.
Bead Cracking--Shows up along edge of flange. Caused by
improper bead attachment, faulty bead or joint compound
application.
`
Wavy Surfaces--Boards are not flat but have a bowed or undulating surface. Caused by improper board fit, misaligned framing, hygrometric or thermal expansion. Also refer to Chap ter 2. Handling and Storage, for proper procedure to keep boards flat before installation.
Board Sag--Occurs in ceilings, usually under high-humidity or moisture conditions. Caused by insufficient framing support for board, board too thin for span, poor job conditions, lack of or mislocaled vapor barrier, or improperly fitted panels. Refer to Chapter 2 for proper job ventilation, storage and frame spacing--particularly with spray-applied texture finishes.
Surface Defects--Fractured, damaged or crushed boards after
application may be caused by abuse or lumber shrinkage. Also see Discoloration below.
Discoloration--Board surface has slight difference in color over joints, supports or fasteners. Caused by improper paint finish ing, uneven soiling and darkening from aging or ultraviolet light.
Water Damage--Stains, paper bond failure, softness in board core or mildew growth are caused by sustained high humidity, standing water and improper protection from water leakage
during transit and storage. Refer to Chapter 2 for proper handling, storage and environmental conditions.
checklist for drywall problems
To find the specific cause for a problem described above, check,
on the following pages, all numerical references listed in the
particular category.
i
fastener impertections joint delects loose panels joint cracking
3,9,10,11.12,22, 23.24, 25,26. 27 1.2,7,8,9.11,13,14,16.19. 20,21 1,3,10, 11,12, 22. 23, 24,25,26, 27 1,11.15.16.17,19
field cracking angle cracking bead cracking wavy surfaces board sag surface defects discoloration waler damage
4 15. 17 15 1.10.16 1.6. 25 4, 5. 8,9 7.8.9 5
GP038 2185
1. PANELS--Improperly Fitted
Cause: Forcibly wedging an oversize panel into place bows the panel and builds in stresses preventing it from contacting the framing (Fig. 1). Result: following nailing, a high percentage of nails on the central studs probably will puncture the paper. May also cause joint deformation.
Remedy Remove panel, cut to fit properly, and replace Fasten Irom center of panel toward ends and edges Apply pressure to hold panel tightly against framing while driving fasteners
Fig. I
2. PANELS--Damaged Edges Cause: Paper-bound edges have been damaged or abused; may result in ply separation along edge or in loosening of paper from gypsum core, or may fracture or powder the core itself. Damaged edges are more susceptible to ridging after joint treatment. Remedy. Cut back any severely damaged edges to sound board before application. Prevention: Avoid using board with damaged edges that may easily be compressed, or can swell upon contact with moisture. Handle Sheetrock Panels with reasonable care.
| J
'
i
Fig 2
3. PANELS--Loosely Fastened Cause: Framing members are uneven because ol misalignment or warping; lack of hand pressure on panel during fastening. Head of fastener alone cannot pull panel into firm contact with uneven members. Also see PANELS--Improperly Fitted.
l-
tuie rontenl may aggravate nail cutting. Raise moisture content ol board and humidity in work area.
23. FASTENERS--Nails Loosened by Pounding Cause Applying panels to the second side of a partition can loosen nails on opposite side. This is particularly true when lightweight, soft lumber, undersized studs or furring are used.
4
Remedy: Check panels for tightness on the partition side where panels were first applied. II looseness is delecled, strike each nailhead an additional hammer blow, being careful to not overdrive the nail. Prevention: Use proper framing. USG Type W Screws or adhe sive application
24. FASTENERS--Nall Pops from Lumber Shrinkage Cause Improper application, lumber shrinkage or a combina lion of both With panels held reasonably tight against framing member and with proper-length nails, only severe shrinkage of the lumber normally will cause nail pops. But if nailed loosely, any inward pressure on panel will push nailhead through its thin covering pad of compound. Pops resulting from "nail creep" occur when shrinkage of the wood framing exposes nail shank and consequently loosens panel (see Lumber Shrinkage de scribed earlier in this chapter).
Remedy: Repairs usually are necessary only for pops which protrude 005" or more from face of board (Fig. 12). Smaller protrusions may require repair if they occur in'a smooth gloss surface or flat-painted surface under extreme lighting condi tions Those which appear before or during decoration should be repaired immediately. Pops which occur after one month s heating or more are usually caused wholly or partly by wood shrinkage, and should not be repaired until near end of heating
season Drive proper nail or USG Type W Screw about 1 'h" Irom popped nail while applying sufhcient pressure ad|acent to nailhead to bring panel in firm contact with Iraming Strike popped nail lightly to seat it below surface of board Remove loose compound, apply finisti coats ol compound and paint
Prevention Proper nail application, use of lumber meeting Framing Requirements (Chapter 2). attachment with USG Type W Screws or by adhesive application (Chapter 2).
GP038
25. FASTENERS--Unseated Nails
Cause Flexible or extremely hard framing or furring docs not permit nails to be properly driven. May result from undersized framing members, type of wood used or supports which exceed the maximum allowable frame spacing
Remedy: Replace nails with 1 'It" USG Type W Screws
Prevention: Use proper framing (Chapter 2). Type W Screws or adhesive application.
26. FASTENERS--Loose Screws
Cause Using the wrong type screw lor the application or an improperly ad|usted screwgun results in a screw stripping or not seating properly.
Remedy: Remove faulty faslener and replace with a properly driven screw.
Prevention: Use USG Screws with combination high/low threads for greater resistance to stripping and pullout; set screwgun clutch to proper depth.
27. FASTENERS--Bulge Around Fastener
Cause: Overdriving fasteners or driving them with the wrong tool can puncture and bulge face paper and damage core of board. Following application of joint compound or texture finish that wets the board paper can result in board bulging or swelling around fastener.
Remedy: Drive screw fastener close to damaged area, clean out damaged paper core, repair with Durabono Joint Compound and refinish.
Prevention: Use correct tool and drive fasteners properly.
Veneer Construction
Many problems associated with veneer construction have the same cause, remedy and prevention as with drywall systems. The similarity appears in application of the base, framing irregu larities, cracking due to structural movement, hygrometric and thermal expansion, and fastener imperlections The additional problems shown below are those specifically relating to veneer finish construction. If solutions to your problems in veneer
-358 problems & remedies
construction are not shown, check similar problems (or drywall construction lound earlier in this chapter.
application 1. MIXING--Foaming Action In Mixer Cause Use of alum as an accelerator when limestone aggre gate is used. Remedy: None--dispose ol batch Prevention: Use moulding plaster or quick-set gauging plaster as an accelerator when limestone aggregate is used. Or, use sand aggregate.
2. SETTING TIME--Variable S(l Time Within Batch
Cause: Insufficient or excessive mixing. Remedy None--dispose of batch.
Prevention: Use proper drill speed; follow recommended mix ing times (see Chapter 2).
3. SLOW SET--DIAMOND Interior Finish Cause: Temperature below 40F. or in excess of 100"F. Remedy None--dispose of batch. Prevention. Avoid extremes of air and mix water temperatures.
4. QUICK SET--DIAMOND Interior Finish a. Cause: Contamination; rusty mixing equipment. Remedy: None--dispose of batch. Prevention Use potable water; clean set plaster residue from equipment after each batch. Always use clean mix equipment. b. Cause- Excessive use of aggregate and/or accelerator. Remedy None--dispose of batch. Prevention. Follow recommendations for mix proportions and use of additives.
5. QUICK SET--IMPERIAL Finish
a. Cause: Excessively low temperatures.
Remedy: None--dispose of batch.
1
Prevention: Maintain min. 55"F air and mix water temperature.
b. Cause Contamination; excessive use of aggregate and/or accelerator
Remedy None--dispose of batch.
Prevention: Same as for Diamond Interior Finish.
veneer application 359
6. WORKABILITY--Stiff Working Cause Mixing action has improper or insufficient shear. Remedy None--use remainder of batch if al all workable. Prevention: Follow recommendations (or mixing time, drill speed and type of mixing paddle (see Chapter 2).
GP038 2187
in-place
7. BOND FAILURE--Delamlnatlon of Finish Coat Cause Basecoal too smooth; finish coat not properly scratched into basecoal to have necessary keying. Remedy: Remove loose material, brush basecoal thoroughly, apply bonding agent and refinish. Prevention: Follow application recommendations (Chapter 2).
8. BOND FAILURE--DIAMOND Interior Finish Cause: Application over faded (not normal blue color) gypsum base. Remedy Remove loose material, brush base clean, apply bond ing agent and refinish. Prevention. Do not store or apply base where it will be exposed to sunlight tor an extended period of time. Where exposed, spray faded base with alum solution before finish is applied.
9. CRACKS--Joint Cracking a. Cause: Imperial Tape overlapped al joint intersections Remedy: Large cracks--apply Perf-A-Tape Reinforcement and USG Ready-Mixed Joint Compound-All Purpose or Taping over the cracks. Minor cracking--flush out area with USG Ready-Mixed Joint Compound-All Purpose. Prevention: Avoid overlapping tape at all joint intersections, including those at angles.
b. Cause. Improper steel stud placement, gypsum base appli cation advanced in wrong direction relative to flange direction Remedy: Repair with Perf-A-Tape Reinforcement and USG Ready-Mixed Joint Compound-All Purpose. Prevention: Install steel studs with all flanges pointing in same direction; arrange gypsum base application so lead edge of base is attached to open edge ol flange first (see No 13 under Drywall Framing Problems )
c. Cause: Overly rapid drying conditions Remedy Repair with Perf-A-Tape Reinforcement and USG Ready-Mixed Compound-All Purpose. Prevention: Liberally sprinkle floor with water to raise humidity
l. I. < ?
Y. ,
s v ijiJ,:$-* -
"
Use Peuf-A-Tape Reinforcement and Durabond Joint Com pound on all joints. Allow compound to dry thoroughly betore applying finish.
10. CRACKS--Field Cracking
Cause Gypsum base installed with vertical joints extending (rom corners ol door and window openings
Remedy Apply Perf-A-Tape Reinforcement and Durabond Joint Compound finished with USG Ready-Mixed Joint Compound-All Purpose, prime and seal (this is a cosmetic treatment, there is no guarantee that cracks will not reopen).
Prevention install USG Control Joints or cut base to (it around openings with joints centered above openings, not at corners.
11. CRACKS--Craze and Map Cracking
Cause: Veneer application too thin. Also can be caused by too rapid drying.
Remedy: Apply spackling putty, prime and seal.
Prevention Apply recommended thicknesses tor both one- and two-coat work. Avoid excessive ventilation which may cause rapid drying When weather is hot and dry, sprinkle floor with water to raise humidity.
12. BLEMISHES--Blistering
a. Cause Loose paper on gypsum base as a result of improper cutting or (rom "peelers" caused by careless handling.
Remedy: Cut and remove unbonded paper, apply bonding agent if gypsum core is exposed, and refinish. Prevention Follow proper handling and cutting procedures.
b. Cause Troweling too early and lack of absorption; excessive material buildup Remedy Minimize troweling and allow finish to become firm. Finish-trowel over freshly set surface to eliminate blisters.
Prevention. Apply material in uniform thickness with minimum amount of troweling to produce smooth surface.
13. BLEMISHES--Joint Ridging and Beading
Cause Joints not preset; excessive ventilation and poor heat control Most likely to occur with one-coat applications.
Remedy. Repair with Perf-A-Tape Reinforcement and USG
Ready-Mixed Joint Compound-All Purpose.
1
Prevention Preset all joints betore veneer finish application; keep ventilation to minimum and control heat In extremely hot. dry weather use Perf-A-Tape Reinforcement and Durabond Joint Compound as alternate joint reinforcement.
14. BLEMISHES--Spalling at Exterior Corners Cause Use ol solid-tlange drywall corner bead Remedy Remove all loose material and corner bead install expanded-tlange corner bead and refmish Prevention Use expanded-llange corner bead
15. STAINS--Staining and Rusting Cause: Use ol improper fasteners, or exposed, improperly pre pared metal trim Remedy Apply rust-locking primer over stains Prevention: Use recommended coated fasteners (see Chapter 1). Apply rust-locking primer to all exposed metal.
16. SOFT. WEAK SURFACE--Dryouts Cause: Too rapid drying conditions Remedy Fog-spray surface with water to provide selling ac tion. When set, apply USG Ready-Mixed Joint Compound-All Purpose for acceptably smooth surface. Prevention: Avoid extending set and/or temperature and hu midity conditions which cause rapid drying.
17. SOFT, WEAK SURFACE-Crumbly Areas Cause: Use ol excessive amount of sand aggregate and/or retarder. Remedy: Treat soft areas with penetrating sealer Prevention: Allow minimum ventilation; use recommended amounts only of aggregate or retarder. Avoid prolonged set
Texture Finishes
U S G texturing materials otter a wide range ol decorative yet practical finishes. Properly used, they can provide interest and variety in decoration while covering minor delects in the base surface. However, certain working conditions, application technigues or equipment problems can cause unsatisfactory results. The following list describes the problem, probable cause and remedy for particular situations.
1. MIXING--Lumping of Wet Mix Cause: Too much water added to initial mix. making lumps difficult to break up. Remedy and Prevention Initial amount ol water added to mix should be slightly less than recommended Alter lumps are broken up. add remaining water.
2. MIXING--Slow Solution Time Cause Insufficient soaking and/or use ol very cold water.
Remedy and Prevention: Allow materials lo soak lor up to two hours, as necessary, if using cold water.
3. MIXING--Wet Mix Too Thin
Cause Addition of excessive water during initial mix Also, insufficient soaking lime in cold water.
Remedy and Prevention: Use recommended amount of water to insure proper consistency. Allow materials to soak up to two hours, if necessary, when using cold water.
4. APPLICATION--Excessive Aggregate Fallout In Spraying
Cause: Excessive air pressure at nozzle, or holding gun too close lo surface being sprayed.
Remedy and Prevention: Use proper air pressure for type of material lo be sprayed; low for Imperial QT Texture Finish, high for USG Spray Texture. (Consult appropriate U.S.G. prod uct data sheet lor recommended air pressure ) Hold spray gun at proper distance from surface lo prevent excessive bounce or fallout of aggregate.
S. APPLICATION--Flotation ot Aggregate
Cause: Overdilution of job mix and/or lack of adequate mixing after water is added to control consistency.
Remedy and Prevention : Add correct amount of water as direct ed on bag to insure proper suspension ol materials in mix. Make certain that water s blended into mix.
6. APPLICATION--Poor Coverage with Spray Finishes
Cause: Not enough water to bring texture material to proper spray viscosity and/or improper application such as moving spray gun too slowly, overloading spray surface and using incorrect spray pressures.
Remedy and Prevention: Add proper amount of water as direct ed on bag. Use correct spray gun pressures and application technique to insure uniform texture with maximum coverage.
7. APPLICATION--Poor Hide
i
Cause Overdilution of mix causing reduction in hiding power.
Insutficient water in spray finishes causes poor material atomi
zation. resulting in surface show-through Also caused by over
extending material or choosing incorrect spray pressures.
Remedy and Prevention: See above.
8. APPLICATION--Poor Bond or Hardness Cause Overdilution ol job-mix results in thinning out ot binder in texture. Contamination or intermixing with other materials can destory bonding power. Remedy and Prevention Add proper amount ot water as stated m bag directions Always use clean mixing vessel and water Never intermix with other products (except tinting materials as recommended)
9. APPLICATION--Stoppage of Spray Equipment Cause: Contamination of material or oversize particles can cause clogging of spray nozzle orihces. Also caused by using incorrect nozzle size for aggregate being sprayed Remedy and Prevention: Prevent contamination during mixing Use correct nozzle for aggregate size ot texture material.
10. APPLICATION--Unsatisfactory Texture Pattern Cause: Improper spray pressures and/or worn spray equip ment. either fluid or air nozzle. Also improper spraying consis tency of mix and/or spraying technique. Remedy and Prevention: Use recommended amount ot water to insure proper spraying consistency. Handle spray equipment correctly lo achieve best results. Make certain that spray acces sories are in good working condition; replace when necessary.
11. APPLICATION--Unsatisfactory Pumping Properties Cause: Mix too heavy. Pump equipment worn or of insufficienl size and power to handle particular type ot texture Remedy and Prevention - Use recommended amount ot water to insure proper spraying consistency. Make sure that equipment is in good repair and capable of pumping heavy materials.
12. APPLICATION--Texture Buildup Cause: Texturing over a high-suclion drywall joint (surface not properly sealed) and/or allowing (oo much time between roller or brush applicalion and texturing operation Overdilution of texture material will produce texture buildup over joint Remedy and Prevention: Seat entire surface with while TAL Alkyd Flat Wall Painf before texture application Use correct amounl ol water when mixing lexlure material and allow safe lime interval between application and final texturing.
13. APPLICATION--Poor Color Match, Ceiling and Sidewall Cause Overspray on ceiling when walls are sprayed with differ ent texture material that is not matched lor color
GP038 2189
362 problems & remedies
2. MIXING--Slow Solution Time Cause Insufficient soaking and/or use of very cold water. Remedy and Prevention: Allow materials to soak for up to two hours, as necessary, if using cold water.
3. MIXING--Wet Ml* Too Thin Cause: Addition of excessive water during initial mix. Also, insufficient soaking lime in cold water. Remedy and Prevention: Use recommended amount of water to insure proper consistency. Allow materials to soak up to two hours, if necessary, when using cold water.
4. APPLICATION--Excessive Aggregate Fallout In Spraying Cause: Excessive air pressure at nozzle, or holding gun too close to surface being sprayed. Remedy and Prevention: Use proper air pressure for type of material to be sprayed, low (or Imperial QT Texture Finish, high for USG Spray Texture (Consult appropriate U.S.G. prod uct data sheet tor recommended air pressure ) Hold spray gun at proper distance from surface lo prevent excessive bounce or fallout ot aggregate.
5. APPLICATION--Flotation ot Aggregate Cause Overdihrion of job mix and/or lack of adequate mixing alter water is aoJed lo control consistency. Remedy and Prevention: Add correct amount of water as direct ed on bag to insure proper suspension of materials in mix. Make certain that water is blended into mix.
6. APPLICATION--Poor Coverage with Spray Finishes Cause: Not enough water to bring texture material to proper spray viscosity and/or improper application such as moving spray gun too slowly, overloading spray surface and using incorrect spray pressures. Remedy and Prevention: Add proper amount of water as direct ed on bag. Use correct spray gun pressures and application technique to insure uniform texture with maximum coverage.
7. APPLICATION--Poor Hide Cause. Overdilution ol mix causing reduction in hiding power. Insufficient water in spray finishes causes poor material atomi zation. resulting in surface show-through Also caused by over extending material or choosing incorrect spray pressures. Remedy and Prevention: See above.
8. APPLICATION--Poor Bond or Hardness Cause. Overdilulion ol job-mix results in thinning out ot binder in texture. Contamination or intermixing with other materials can destory bonding power. Remedy and Prevention: Add proper amount ol water as stated in bag directions Always use clean mixing vessel and water Never intermix wilh other products (except tinting materials as recommended).
9. APPLICATION--Stoppage of Spray Equipment Cause: Contamination of material or oversize particles can cause clogging of spray nozzle orifices. Also caused by using incorrect nozzle size for aggregate being sprayed. Remedy and Prevention: Prevent contamination during mixing Use correct nozzle for aggregate size ol texture material.
10. APPLICATION--Unsatisfactory Texture Pattern Cause. Improper spray pressures and/or worn spray equip ment, either fluid or air nozzle. Also improper spraying consis tency of mix and/or spraying technique. Remedy and Prevention: Use recommended amounl of water lo insure proper spraying consistency Handle spray equipment correctly to achieve best results. Make certain that spray acces sories are in good working condition; replace when necessary.
11. APPLICATION--Unsatisfactory Pumping Properties Cause: Mix too heavy. Pump equipment worn or ol insulticient size and power to handle particular type of texture Remedy and Prevention: Use recommended amount of water to insure proper spraying consistency. Make sure that equipment is in good repair and capable of pumping heavy materials.
12. APPLICATION--Texture Buildup Cause: Texturing over a high-suction drywall joint (surface not properly sealed) and/or allowing too much time between roller or brush application and texturing operation Overdilution of texture material will produce texture buildup over |Oint Remedy and Prevention Seal entire surlace with white TAL Alkyd Flat Wall Painl before lexture application Use correct amount ol water when mixing texture material and allow sale time interval between application and final texturing
13. APPLICATION--Poor Color Match. Ceiling and Sidewall Cause Overspray on ceiling when walls are sprayed wilh dillerent texture material that is not matched for color.
364 'problems & remedies
Remedy and Prevention Use color-matched USG Spray Tex ture (or sidewalls with Imperial OT Texture Finish tor ceilings. (Paint added at job to either wall or ceiling texture can cause color dilference )
14. FINISH SURFACE--Poor Touchup Cause It is very difficult to touch-up a textured surface to completely blend with the surrounding texture. A conspicuous touchup is caused either by texture or color variance. Remedy Perform touchup operation with extreme care; other wise. re-texture entire wall or ceiling area.
15. FINISH SURFACE--Joint Show-Through
Cause: Overlhmned or overextended texturing material does not adequalely hide the normal contrast between joint and gypsum panel paper Also caused by improperly sealed surface.
Remedy Use correct amount ol water when mixing texture material and apply at recommended rale of coverage until joint is concealed
Prevention Seal entire surface with white TAL Alkyd Flat Wall Paint before texture application.
16. FINISH SURFACE--White Band or Flashing Over Gypsum Panels
Cause: High-suction gypsum panel joint causes a texture varia tion which often appears as a color contrast.
Remedy: Allow texture to dry. and paint entire surface.
Prevention Seal entire surface with white TAL Alkyd Flat Wall Paint before spray texture application.
17. FINISH SURFACE--White Band or Flashing Over Con crete
Cause Damp concrete surface on which leveling compound has dried completely can produce results similar to those of high-suction joint.
Remedy: Allow texture to dry, and paint entire surface.
Prevention Allow concrete to age for at least 60 days for complete dryout; then seal with TAL Alkyd Flat Wall Paint before applying texture
18. FINISH SURFACE--Joint Darkening
,
Cause Application over damp joint compound, especially in cold, humid conditions.
Remedy: Allow texture to dry completely, and paint entire surface.
Prevention Seal surface with white TAL Alkyd Flat Wall Paint betore texture application.
fJISSiCt p/t'Cdl/IIOIIy JU J
Conventional Plaster Construction
'All USG basecoal and finish plasters are carefully manufac tured and thoroughly tested belore shipment Along with the functional characteristics provided, U S G plasters are carefully formulated for use under normal, prevailing weather conditions and with aggregates commonly used in Ihe market
Plasters are adversely allected by aging and abnormal storage conditions, use of Ihe wrong aggregate and improper proportioning--all ol which may allect Ihe set. hardness and working properties ol the material. Most plaster problems result Irom Ihe following situations.
1. Adverse atmospheric and |ob conditions 2. Set conditions--too fast or slow 3. Poor quality and incorrect proportioning of aggregate. 4. Improper mixing, application or thickness of basecoal or finish 5. Incorrect lathing practices 6. Dirty or worn mixing or pumping equipment.
Basecoal and finish coat plasters are so closely interrelated lhal problems pertaining to their use are treated together No at tempt is made here to discuss problems lhal might occur due to structural deficiencies. These have been covered earlier in this chapter. Plaster problems are classified under the specific type of condition which exists. These are discussed in order, in the following groups:
1. Plaster cracks. 2. Blemishes, color variation, surface stains. 3. Weak, soft walls. 4. Bond failure. 5. Set and working qualities. 6. Gauged lime putty problems.
1. CRACKS--Connecting vertical, horizontal cracks at some what regular intervals, often in "stepped" pattern, also diagonal. Material--Plaster over metal or gypsum lath.
a. Cause: Plaster loo Ihm, insufficient plaster grounds
Remedy: Patch. Prevention: Apply plaster to proper thickness.
b. Cause: Weak plaster (through dryout or slow set)
Remedy: Spray with alum solution to accelerate set.
Prevention Add accelerator to plaster mix to bring setting time to normal range.
c. Cause: Excessive use of aggregate. Remedy: Patch. Prevention: Use proper proportions of aggre gate and plaster.
d. Cause: Failure to use Slriplath reinforcement at potential weak points
Remedy: Cut out, reinforce and repair.
Prevention: Install proper reinforcing.
366 problems & remedies
e. Cause: Expansion ol rough wood frames. Remedy Remove plasler and lath as necessary. Seal frames and patch. Prevention Seal frames Cut basecoat along grounds prior to sel install control joints over frames.
Material--Plaster over unit masonry. Cause Structural movement of masonry units Remedy and Prevention: Correct masonry construction, install control joint, patch.
Material--Plaster over brick, clay tile or concrete block at door openings Cause: Poor lintel construct n. improper frame construction. Remedy Patch. Prevention: Use proper frame and lintel con struction with self-furring metal lath reinforcement.
2. CRACKS--Fine cracks, random pattern, generally I" to 3" apart Includes shrinkage cracks, crazing, alligatoring, chip cracks Material--Gauged lime putty finish over gypsum basecoat. used with any plaster base. Cause Insufficient gauging plaster--shrinkage of lime Insuffi cient troweling during setting. Applied finish too thick. Basecoat too wet or too dry and too little or too much suction. Remedy: Apply spackling putty and primer-sealer. Prevention: Use sufficient gauging plaster, trowel sufficiently, or properly condition basecoat before applying finish.
3. CRACKS--Fine cracks, irregular pattern, generally 6' to 14" apart, "map cracking". Material--Trowel finishes over gypsum basecoat--unit masonry plaster base. a. Cause: Finish coat applied too thick. Remedy: Patch. Prevention: Apply finish coat to Vi" thickness but not more than V".
b. Cause: Improper timing of final troweling Remedy Patch. Prevention: Water-trowel as final set takes place (not before) to provide dense, smooth surface.
c. Cause Retempering gauged lime putty. Remedy Discard batch; make up new gauge. Prevention Gauged lime putty should not beretempered once it has started final set.
4. CRACKS--Random pattern, usually less than 12" apart, called map. shrinkage or fissure cracking. Material--Basecoat over masonry.
plaster cracks 367
a. Cause High suction of masonry base Remedy: II bond to base is sound and cracks are open or more, fill by troweling across cracks with properly aggregated plasters. If bond is sound, finish over fine cracks with highly gauged trowel finish or float finish. If curled at edges and bond is unsound, remove and reapply using proper plaster method. Prevention Wet masonry with water to reduce suction before basecoat application.
b. Cause: Under-aggregating of basecoaf; slow set Remedy: Same as above. Prevention: Use 3 cu ft. of aggregate per 100 lb. gypsum plaster (see Chapter 4 for proper proportion of aggregates). Discontinue use of job-added retarder and accelerator, it necessary, to obtain proper set.
c. Cause: Dryout condition. Remedy: Spray basecoat either with water or alum solution to thoroughly wet plaster. Proceed same as above. Prevention: In hot, dry weather, protect plasler from drying loo rapidly before set. Spray plaster during set time if necessary.
5. CRACKS--At wall or ceiling angles. Material--Plaster over gypsum lath. a. Cause: Thin plaster. Remedy: Cut out and patch. Prevention: Follow correct appli cation procedure. b. Cause: Failure to use Cornerile reinforcement Remedy and Prevention: Same as above.
6. BLEMISH--Water-soluble, powdery crystals on surface, gen erally white but may be colored. Can be brushed ofl. Material--Basecoat and finish plaster over concrete block or clay tile. Cause: Efflorescence. As masonry units dry, water-soluble salts from units or mortar joints leach out and are deposited on the plaster surface. Remedy: After plaster surfaces are thoroughly dry. brush oft efflorescence, apply oil-base sealer and paint Prevention: On interior walls, eliminate source of moisture, remove efflorescence belore plastering, decorate with oil-base sealer and paint. On exterior walls, eliminate moisture source, fur out. lath and plaster.
7. BLEMISH--"Pops", peak-like projections which tall out and create little craters or pits; often with fine radial cracks. Material--Gauged lime putty finish. a. Cause: llnslaked lime in mortar which slakes and swells after it is applied.
jdo prooiemi & remedies
Remedy Remove core of "pops" and patch after popping has ceased Prevention: Allow sufficient soaking tim. or normal hydrated lime, or use double-hydrafed lime or a prepared finish such as Red Top Finish Lime.
b. Cause: Contamination from foreign matter. Remedy: Same as above. Prevention: Eliminate source of im purity
Material--Gypsum basecoal and finish.
Cause: Lumpy or undissolved retarder added on job Retarder lumps swell or "pop " when wet.
Remedy: Cut out spots and patch.
Prevention: Completely disperse retarder before adding to mix
water; mix well to distribute retarder throughout plaster.
1
B. BLEMISH--Blisters in finish coat occur during or immediate ly after application.
Material--Gauged lime putty finish a. Cause Base too green (wet); insufficient suction; too much water used in troweling.
Remedy Alter finish has set. trowel with very little water. Prevention: Do not apply finish coal over green basecoat.
b. Cause: Finish too plastic.
Remedy: Same as above. Prevention: Add small amount of very line white sand to putty, or increase amount of gauging plaster.
9. BLEMISH--Excess material ("slobbers' ) on finish surface. Material--Gauged lime putty (inish.
Cause. Improper joining technique, excessive or improper troweling leaves excess material on finished surface.
Remedy Scrape ott excess material before decoration. Seal surface when plaster is dry.
Prevention: Previously applied finish should be cut square for completion ot finish. Avoid excessive troweling at joining
10. BLEMISH--Peeling paint.
Material--Gauged lime putty finish.
a. Cause Paint applied over wet plaster.
Remedy Scrape oil peeled paint, allow plaster to dry, and
redecorate.
(
Prevention Be sure plaster is dry before decorating, and use a breather-type paint.
b. Cause Weak finish Plaster worked through set Remedy Scrape oft peeled paint, patch and decorate. Prevention Do not retemper or trowel finish alter set.
p/UMtl' Vdl UlOU/l^
joa
11. COLOR VARIATIONS--Streaks and discoloration
Material: Lime finishes, gauged with gauging plaster or Keenes Cement
e. Cause Lime and gauging plaster not thoroughly mixed.
Remedy Seal and decorate Prevention: Follow recommended
mixing procedures.
b. Cause Too much water used in troweling
Remedy: Same as above. Prevention: Apply as little water as possible in troweling.
c. Cause: Dirty tools or water.
Remedy: Same as above. Prevention: Wash toots and use clean water.
j >
i
------------------------------------------------------------- ,--,----- .---------------
12. COLOR VARIATIONS--Light and dark spots
j
Material--Float (inish.
,
a. Cause Improper technique or too much water used in lloating.
-
Remedy Seal and paint to gel uniform color
Prevention: Follow recommended application procedures
b. Cause Spotty suction on basecoatwhich wasdampened unevenly by throwing water on with a brush rather than by spraying with a tine nozzle.
Remedy: Same as above. Prevention: Dampen basecoat uni formly using a tine spray.
i
13. COLOR VARIATIONS--Light or tlat spots in light-color paint. Material--Oil paint over gauged lime putty finish
Cause' Surface painted loo soon after plastering (alkali in lime saponifies paint); paint pigments not limeproot. Remedy and Prevention: Apply primer-sealer and repaint.
Material--Any colored paint over any plaster finish.
Cause: Non-unilorm absorption results in uneven surlace gloss and coloration. Remedy and Prevention Apply primer-sealer and repaint
14. SURFACE STAINS: Yellow, brown or pink staining-- "yellowing".
Material--Any lime putty finish over any basecoat and plaster base, generally occurs while surface is damp.
a. Cause Contaminated aggregate.
Remedy: Apply primer-sealer and repaint
Prevention Use clean aggregate
r
b. Cause: Smoke lumes (rom gas healer. Remedy: Same as above. Prevention- Vent heaters to outside.
c. Cause: Tarpaper behind plaster base; creosote-treated fram ing lumber; tar or tar derivatives used around job; sulphur or chemical lumes. Remedy Same as above. Prevention: Use asphalted paper. Remove source ol air contamination.
15. SURFACE STAINS--Rust. Material--Plaster over any plaster base. Cause- Rusty accessories; or any protruding metal. Remedy Apply primer-sealer and decorate. Prevention: Use accessories made ot zinc alloy or with hot-dip galvanizing. Do not use accessories that show rust prior to installation.
16. SOFT WALLS--Soft, white, chalky surfaces, occurring dur ing hot, dry weather, usually near an opening.
Material--Gypsum basecoat over any plaster base.
Cause: Dryout. Too much water has been removed before plaster can set.
Remedy Spray with alum solution or plain water to set up dryout areas.
Prevention- Screen openings in hot, dry weather; spray plaster during set; raise humidity by sprinkling floor with water.
17. SOFT WALLS--Solt, dark, damp surfaces occurring during damp weather.
Material--Gypsum basecoat over any plaster base.
Cause- Sweat-out. Too little ventilation allowed water to remain in watt (or an extended period after plaster set. Some plaster has re-dissolved.
Remedy: Dry walls with heat and ventilation. It sweat-out condi tion continues, there is no remedy; remove and replaster.
Prevention- Properly heat and ventilate during plastering.
18. SOFT WALLS--Soft, dark, damp surfaces, occurring in
treezmg weather.
1
Material--Gypsum basecoat over any plaster base.
Cause Frozen plaster.
Remedy: It plaster freezes before set, no remedy except to remove and replaster.
Prevention Close building, supply heat.
plaster failures 371
19. SOFT, WEAK WALLS--General condition, not spotty or due to slow set. Material--Gypsum basecoat over any plaster base Cause Too much aggregate or line, poorly graded aggregate
Remedy No remedy, remove and replasler.
Prevention: Use properly graded aggregateand correct propor tioning.
20. WEAK WALLS--Weak plaster.
Material--Gypsum basecoat.
Cause: Extremely slow set.
Remedy: Spray with alum solution to accelerate set
Prevention: Add accelerator to plaster mix to bring setting time
within normal range.
:
Material--Gauged lime putty finish over any basecoat.
Cause: Too little gauging with iHuitficient troweling, retemper
ing, basecoat loo wet.
^'
Remedy: No remedy; remove and replasler.
Prevention: Use proper ratio of gdW|rncf fo lime putly Do not relemper plaster. Trowel adequately to assure desired hardness.
21. BOND FAILURE--Basecoat separation. j.
Material--Gypsum basecoat over gypsum of Ihelal lath
Cause: Too much aggregate, plasteb'application over frost on lath, freezing ot plaster belore set, or addition ot lime or Portland cement. Excessive delay in plaster application after mixing, extremely stow set or retempering.
Remedy: No remedy except to replaster.
,
Prevention- Provide proper job conditions during plastering. Follow correct mixing and application procedures.
22. BOND FAILURE--Brown coat separation trom scratch coat. Material--Gypsum basecoat plasters. a. Cause: Weak scratch coat. Remedy: None; remove and replasler Prevention: Use proper aggregate amount Avoid retempering
b. Cause: Failure to provide mechanical key in scratch coal. Remedy Roughen scratch coal and replasler. Prevention Cross-rake scratch coal to provide rough surface tor brown coat
a. Cause: Dryout ot scratch coal Remedy: Water-spray scratch coat lor thorough set before brown coat application.
Prevention Provide proper job conditions during plastering, screen openings in hot, dry weather. Water-spray plaster during set Raise humidity by sprinkling lloor with water
23. BOND FAILURE--Finish coat separation. Material--Gauged lime putty finish applied over gypsum brown coat. a. Cause Brown coat too smooth, too dry, wet or weak, limsh improperly applied; incomplete hydration ot linish lime. Remedy and Prevention Where brown coat is cause, strip ott finish, correct condition ol brown coat and replaster. Where finish is cause, remove it and refinish using properly propor tioned double-hydrated lime or a prepared finish.
b. Cause. Frozen finish coat. Remedy and Prevention: Remove finish, provide sufficient heat during plastering, reapply finish.
24. SLOW SET--See Soft. Weak Walls.
25. QUICK SET--Plaster sets belore it can be properly applied and worked Material--Gypsum basecoat over any plaster base. a. Cause: Dirty water, tools or mixing equipment, or excessive use of accelerator. Remedy Discard material as soon as it begins to stiffen; do not retemper. Prevention: Use clean water, tools and equipment.
b. Cause Mixing too long. Remedy: See above. Prevention: Reduce mixing time.
c. Cause Poor aggregate. Remedy: See above. Prevention: Use clean, properly graded aggregate or add retarder.
d. Cause Error in manufacture. Remedy: See above. Send samples to manufacturer's repre sentative. Prevention: Add retarder.
e. Cause. Machine-pumping and application that exceed limits of time and distance pumped for plaster being used. Remedy: See above. Prevention: Add retarder. Use plaster de signed for machine application.
26. ERRATIC SET--Lack of uniformity in set. i Material--Gauged lime putty over gypsum basecoat. Cause. Variable temperature. Remedy and Prevention: Maintain uniform job temperature. In cold weather, heat building to min. 55F.
27. POOR WORKING--Works hard or short", loses plasticity and spreadability Does not carry proper amount ol aggregate Material--Gypsum basecoat over any plaster base a. Cause: Aged or badly stored plaster Remedy Obtain Iresh plaster and mix equal parts with aged plaster, or use less aggregate. Prevention: Use fresh plaster
b. Cause Over-aggregaling. Remedy: None Prevention: Use proper proportioning Material--Gauged lime putty over gypsum basecoat. a. Cause: Aged lime, partially carbonated, warehoused loo long or improperly. Remedy: None. Prevention: Use fresh material
b. Cause: Improper soaking, slaking Low temperature during putty preparation Remedy None. Prevention Use proper lime putty preparation procedure. Do not soak at temperatures below 40'F
28. SOUPY LIME--Material loo fluid for proper gauging and application. Material--Lime putty. a. Cause: Soaked too wet. Prevention: Follow directions for type of lime being used
b. Cause: Cold weather, cold mixing water. Prevention: The gelling action of lime is retarded when material is soaked in temperatures less than 40F. with cold water. Use warm water to quicken gelling.
29. LUMPY LIME--Material too lumpy for proper blending with gauging plaster. Material--Lime putty. a. Cause: Old lime. Prevention: Use fresh lime.
b. Cause: Damp lime. Prevention: Protect lime from moisture on job and in storage.
c. Cause Incorrect soaking Prevention: Follow soaking directions for type of lime used.
d. Cause: Excessive evaporation Prevention: Cover lime box with tarpaulin to reduce evapora tion.