Document 70R1Nnnnw9bD0NqkZkNR09MoB
CAMBRIDGE
'*0.1 t i I 4
TO: "E. S. Wood
FROM: J- c. Yang
DATSUBJECT:
cc.- R. M. Vining
H. C. Duecker
B. R. Williams H. A. Eschenbach
J. W. Wolter
B. A. Blessington
W. R. Hanlon
C. C. Ou
D. M. Kirven
F. W. Eaton
R. C. Ericson 0. M. Favorito
R. H. Locke
S. C. Vaughan
File: 71-048/049 V
May 16, 1977 Tremolite & Vermiculite Content in Libby & Kearney Ore Deposits
and Expanded Vermiculites
,, PLAINTIFF'S EXHIBIT
WRG-1580
OBJECTIVE
The objective of this study is to determine the vermiculite and tren*olite content in ore concentrate and expanded vermiculite from the Libby land Kearney mills. A sample of the head feed from the Libby mills, from which all the Libby ore samples were derived, is also analyzed as a check for the effectiveness in fiber removal of the Libby operation.
The samples analyzed below are single samples of concentrate or ex panded product, selected at random. We do not know how accurately these samples represent the average with respect to tremolite (or amphibole min eral) content. Further sampling will be required to better establish more typical or average values.
The reported tremolite content may include other amphibole minerals, particularly hornblende, which cannot be distinguished from tremolite.
SAMPLE DESCRIPTIOH
All -the analyses made in this report were single sample analyses. From the materials submitted in 5-10 lb. quantities, they were quartered very carefully and repeatedly until the desired sample sizes (200-300 grams) were obtained, which were expected to be fairly representative. However, the range of variations in field sampling and in the geological formations were not established, so that the results observed may only indicate a ballpark figure with 10j( of accuracy.
WR0012427 15032158
To: From: Date:
E.S.V."3od J.C.Yang Kay 16, 1977
rrenolit-i i Veraic.'.
iiiboy
'/ v*
one i sanded Vernicu
oasu; `7?
ID Wo.
99952-31 99952-32 99952-33 99952-3^
99952-35
99952-36 99952-37 99952-38
99952-39 99952-40
99952-48
99952-41 99952-42 99952-43
99952-46
Description
Date and Source
Ore Concentrate Ore Concentrate Ore Concentrate Ore Concentrate
L-l L-2 L-3 L-4
3/10/77 - R. L. Oliverio
Ore Concentrate L-5
3/1/77 - E. D. Lovick
Ore Concentrate Ore Concentrate Ore Concentrate
K-3 K-4 K-5
3/7/77 - 0. F. Stewart
Expanded Vermiculite L-l Expanded Vermiculite L-2
3/21/77 - F. W. Eaton
Expanded Vermiculite L-3 (Terra-Lite)
Expanded Vermiculite Expanded Vermiculite Expanded Vermiculite
K-3 X-4
K-5
3/9/77 3/3/77
- F. W. Eaton
*
-r
- 0. F. Stewart
Libby Head Feed - a composite of 3 shifts
3/9/77
- R. L. Oliverio
METHOD
1. Tremolite Analysis of Libby #1 and #2 Concentrate:
Since the fiber bundles and the rock aggregates are unusually large, tremo lite fiber bundles and rocks were first separated by hand-picking of a carefully, quartered sample. The vermiculite was then separated from the rock by screening; Rocks and fines in the -50 mesh fraction were x-rayed for quantitative determination of treroute. The total tremolite was obtained as'the sum of factored portions from hand-picked and the fine portions. The scheme of analysis is shown in Figure 1.
2. Tremolite Analysis of #3 Ore Concentrate:
The concentration of rock fines and tremolite fiber fractions are shown in Figure 2. Vermiculite was separated by chemical exfoliation with 30% #2^2* followed by water flotation.
WR0012428
15032159
To: From Date
E.S.Wood J.C.Yang May lo, 1977
3. Tremolite Analysis of #4 and #5 Ore Concentrate:
A set of finer screens than the ones used in analyzing #3 ore was selected for this separation. A diagram of the procedure is shown in Figure 3*
4. Tremolite Analysis of Expanded Vermiculite (size #2 to #5)
The expanded vermiculites are easier to work with since they were expanded already pd the percentage of rocks and fines were lower than those of the corresponding ore concentrates. The procedure for analyses is shown in Figures 4 and 5> respectively.
5. Tremolite Analysis of the Head Feed:
The head feed sample from the Li'oby mill was obtained one day before the ? ore composite collection from the screening plant, and is the starting ) material from which the ore composites were obtained. The analysis was more complicated than the others since the size varied over a wide range and the non-vermiculite portion was very high. The tremolite concentration procedure is shown in Figure 6.
6. Vermiculite Analysis of Ore Concentrates:
To cross-check the vermiculite analysis from the scheme shown in Figures 2 and 3j for ore composites #3 and #5, a 100 g ore sample was taken and expanded in a furnace for 5 minutes at 1?00F., then allowed to cool at ambient conditions for half an hour. In general, a weight loss of about 7% resulted from heat expansion. By previous experience, a higher vermiculite yield will result from chemical expansion since some of the poorly weathered vermiculite will not readily respond to heat expansion but will expand in H202. The complete analyses of the Libby and Kearney vermicu lites are. shown in Tables 1 and 2.
7. Evaluation <ST Fine Fiber Content:
In Table 1) a breakdown of the tremolite fiber in ore concentrate by size fraction is also shown. The fines (-50M for size L-l to L-3; -100M for size L-4 and L-5) can be considered to be the mavimnm limit of the res pirable fiber portion (provided no further vigorous mechanical degradation of the material takes place in handling).
We have also hand-picked the fiber bundles from two L-2 ore concentrate samples and run the.r. through the air-elutriation column built in the lab oratory. We then collected the airborne particulate through a series of screens and then on a wet filter under vacuum. The screens used were graded to eliminate the blockage of the filter by large dust aggregates and long fibers. This experiment indicated the fiber bundles were fairly stable. At the end of 30 minutes of the air elurriation, the results are as follows:
WR0012429
o
o
To: E.3.Wood From: J.C.Yang Date: May 16, 1977
-u-
Tremolite & Verniculire Content, in Libby & Kearney Ore Deposits
and Expanded Vermiculites
Sample Description
Tremolite, hand-picked from SL-2
Tremolite, hand-picked from CL-2
$ vt. on 325 mesh screen
0.29
0.21
$ wt. on wet filter
0.05
0.04
Respirable Dust
0.34
0.25
Observation:
mostly fiber some larger than 30 ji
fiber and vermiculite
dust
The fine sized dust content average for the two samples was approximately..
0.3$, corresponding to .0076$ of the total sample. Thus, it is concluded that
the amount of respirable size tremolite fiber present in the L-2 ore composite
must be less than 0.01$.
f
No attempt was made to determine the respirable size fiber content from the Kearney ore since most of the Kearney tremolite is massive and difficult to be distinguished from hornblendes present.
In the expanded product, the tremolite fiber contents found in the Libby ventriculites as shown in Table 2 were primarily fine sized. Very few small bundles were observed which demonstrates the effectiveness of fiber removal by the stoner.
COMMENTS
1. The tremolite content of L-l and L-2 were reduced to about half the amount of those analyzed in 1976 (see Research Report on Libby Ore Evaluation J. C. Tang to H. C. Duecker, 2/23/76). The tremolite content of L-3 and L-4 has apparently not improved since early 1976. However, the vermiculite platlets were much cleaner presently with less dust particles adhered to the surface than those of 1976.
2. This is the first time that Kearney ores and expanded vermiculites of all sizes were analyzed for their total tremolite content by the x-ray diffrac tion method. Unfortunately, the x-ray diffraction patterns of the fibrous and massive forms of tremolite are identical and in fact cannot be distin guished from other amphibole minerals, particularly hornblende. More sophisticated analytical methods using electronmicroscopic techniques and related structural and elemental analysis such as TEM, SEM, SAED and EDAX are needed to pinpoint the exact nature of the amphibole minerals present.
vjroi243
15032161
From: J.C.Yang Date: May lo, 1977
.o
ana Zxoar.ded Ve:
* -- --
TA3I Tresolite Content of Ore Concentrate
0Jti4 ;i?:
ID No. -31
Description L-l
Date 3/10/77
Vs. 91.7
Tre aolite
(+50M) (-50M)
1.2 .00?
^ Total Treaoli-ce*
1.2
-32
L-2
3/10/77
91.2
(+50M)
2.5
(-50M)
.018
2.5
-33 L-3 -3^ L-4
-35 -36 -37
L-5 K-3 K-4
-38 K-5
-46 Head Feed, Libby " -
3/10/77 3/1/77 3/1/77 3/1/77 3/1/77 3/1/77 3/9/77
78.1
(+50M) (-50M)
.653 .013
70.1
(+7QM) (-70 +100M)
(-10014)
1.495 .232 .009
63.9 72.0
(+70M) (-70 +100M)
.119 1.016
1.913
(+50M) (-50M)
1.60 .158
75.1
(+7CM) (-70 +100M)
(-10QM)
8.903 .554 .492
76.6
** 7*0
(+7CM) (-70 +10QM)
(-100M)
0.874 2.070 13.034
(+6m) (-6 +20tM) (-20 +70M)
(-70M)
1.302 .684
1.235 .609
0.7 '%
l.t 'r
3.0 1.8
10.0
15.9
2J3
Includes all amphibole minerals. The material floated after expanded with 30$ HgOg.
CONFIDENTIAL:
WR0012432 15032163
To I O * i* oo cl From: J.C.Yang Date: May 16, 1977
in Libby & Kearney >-a Dero3it3 and Expanded VerrJ.cu2J.te
TABLE 2 Treoolite Content of Expanded Veraiculite
ID No. 99952-39 99952-40 99952-48 99952-41 99952-42 99952-43
Description L-l L-2 L-3 K-3 k-4 K-5
Date Collected
3/18/77
3/18/77 3/9/77 3/3/77 3/3/77 3/3/77
* Veraiculite
97.7
97.1
97.7
91.0
% Tremolite
0.074
0.028 .
0.049^ 'r
1.6
79.4 48.7
ft
interference
Includes all amphibole minerals.
ONFiDENTIAL
WR0012433 15032164
i' tremolite analysis of -i m =.2 :==: sjm?-.s;i-S
Sanpis (200 g) i=l or =2 1 har.d picking
^ /Sj
J.C-.Yang:nlr
5/16/77
WR0012434 15032165
?.) TREMDLITE ANALYSIS Y? .=?. :\RY C?:?C3I'ZE
Smple ?t3 f!50g)
Oo'crll i bvj
Oven dried
JI 110C/U-6 hours
filtered dried
I filtered | dried
weighed
weighed
ITMV
Via -rayed Tremolite
30^ H202 Oven dried 110oC/t-6 hours
weighed
x-rayed
TrenoLite
5/16/77
WR0012435 15032166
3) TRZMOLITE ANALYSIS
ar.d =? '? COMPOSITE Saaple ' 15- g)
f 1J`
-1.4A
J.C.Yangrmlr
5/16/77
15032167
Expanded Ver.-ruiculite (250 g)
Va filtered dried weighed
v
Vn
J.C.Yangimlr 5/16/77
Heavy Fraction
Va and soma fines mostly rochs and fines
filtered
filtered
washed
washed
dried
dried
x-rayed *
x-rayed
Tremolite
Tremolite
\/
\^
factored
factored /
\/
sun
Total Trsnolite
WR0012437 15032168
5) TRESiIS5 ANALiSlS 1? ^ iSr/uCSD VIIvLICULIII Expanded Vera (250 ^5
OJti-U
Vm
^filtered juried ^weighed Vm
Heavy Fraction filtered dried and weighed x-rayed
Tremolite Content factored
Total Tremolite
J.C. Yangrmlr
5/16/77
UK0012438
15032169
6) TREMO LIT! ANALYSIS
3Z :Z.-Z FELL
A-head feed from Libby v;-.3 analysed from which "he L-l, L-2, L-3 and L-U were obtained.
Head Feed ' ~ ~iO 5) I screening
composite Ojlvl 1 / l/v)