Document 6pZx9b8rLmqy1R3yjYaYRe26
MONSANTO CHEMICAL COMPANY
10-1-44
SALESMEN'3 MANUAL
AROCLOR
DESCRIPTION AND PROPERTIES
The Aroolors are a series of chlorinated hydrocarbons based on biphenyl and terphenyl. They are not pure compounds but are
mixtures of olosely Telated chlorine substitution products man ufactured essentially to a set of specifications based on physical properties rather than chemical composition.
The approximate chlorine content is indicated by the last two
figures of the Aroclor number. The chemical composition closely approaches the average for the indicated chloro-derlvatlves as follows,but should not be represented as simple chemical compo sitions according to the formula shown:
Approximate Equivalent Chemical Compound
1239+1
1232 1242 1248 1254 1260
1262 1268 1271 5460
Monochloroblphenyl Dlchloroblphenyl
Trlchloroblphenyl Tetrachlcroblphenyl Pentachloroblphenyl Hexachloroblphenyl Heptachloroblphenyl Nonachloroblphenyl Decachloroblphenyl Nonachloroterphenyl
Reference should be made to technical bulletin P-115 for tables and graphs of physical properties. This manual contains only that information which is not designed for general public distribution or has been made more recently available than permitted incorpora
tion in the printed bulletin.
The following Aroolors not in commercial production (but available) have been proposed:
Aroclor No.
5448
5454
Fixed Chlorine Polor (I.ovlbond)
Pour Point Softening Point
47.9# 6.0
60C
63C
54.83# 20.0 84C
85C
09^643
mqns
MONSANTO CHEMICAL COMPANY
10-1-44
Aroolor No.
5448
5454
Viscosity 98.9OC (210P) 395-0* -
Flash Point Burn Point
250C 400C
-
Chlorides Acidity - mg. KOH/g.
None 0.008
None 0.004
Evaporation
0.006
0.007
Resistivity Ageing Dlelectrlo Constant
SOS
4.65
4"iO
ELECTRICAL PROPERTIES
4***" ftr^/ Aroclor Aroolor Aroclor Arcelor
l^v ,-<v 1248
1254
1260
5442
Dielectric Constant 9 ii>fo tf-1 4.63 4.15-4.35 3*6-3.8 4.92
Resistivity 9 100C, OHMS/Cm3 500x10? Above,, Above 1469x10?
, ft. tat AO.
i00xl09 500x10?
Dielectric Strength
3^KV Min.
Power Factor (100C, 1000 kc) Less than 0.1#
Less than 0.13C
IRS Method H-3955871
Resistivity 9 100 under 500 Volts DC
ASTM D.177-11
.
Refractive Index
Range
Aroclor 1270
Aroclor 1271 Tetradecaohlorometaterphenyl Tetradecaohloroparatorphenyl
1.691-1.74 1.691-1.74
1.712-1.718 1.691-1.74
Heat of Vaporization
Aroolor 1260 (3 bob. pressure) ' Aroolor 1262 (760 mm. pressure)
Aroclor 1169 (0.151 atBi, 9 350C) (0.079 atm. 9 325C)
Midpoint
1.712 1.712
1.712
B.IU/lb.
104 72.4 69.2 70.6
2- MOhS 09Z644
MONSANTO CHEMICAL COMPANY
10-1 -44
SOLUBILITY
Solvent
Acetone Alcohol, Formula 3-A Amyl Acetate Amyl Alcohol Benzene Butyl Acetate N. Butyl Alcohol Carbltol
Chloroform D1 Butyl Phthalate Ether Ethyl Acetate Ethyl Lactate Ethylene Bichloride 40% Formaldehyde Furfural High Test Gasoline Glycerin Kerosene Linseed Oil Methyl Acetate Mineral Spirits Paraffin Phenol 90% Pine Oil Pyridine Toluene Trl Cresyl Phosphate Tung Oil Turpentine Xylene
Aroelor 1268
Cold
Hot
I
I S 8
8
S PS
s
70
S
3 S PS s
s
I
PS
I
s s
PS
.
3 s
s s
s 3
JVC
I . Insoluble PS Partially Soluble
S Soluble
Solvent
Gas.. Aroolor 1270 per 100 cc.Solvent
Approx. Temp, at vhlch soln.oomplete
Furfural Furfural Secondary Amyl Acetate Secondary Amyl Alcohols
Carbltol Heavy White Mineral Oil
2.0 4.0 4.0 4.0
4.0 4.0
105-110OC 120-125C 110-115OC Not completely soluble at boll
Above 125C
110-115C
~ MONS 091645
Toward Heat
MONSANTO CHEMICAL COMPANY STABILITY
'
10*1-44
Aroclor 1248 was heated to 650P In stainless steel autoclave with the resulting changes indicated In the following tabulation:
Original Sample Autoclave #1 Autoclave #2
Autoclavo #3
Time of Heating (Hours)
0 331 500 669
Temper ature
343C. 6500?. 343C. 650F. 3430C. 650?.
.0021
.0392 .0809 .0800
Those results are interpreted as indicating very .excellent stabil
ity for Aroclors under the conditions of test.
`
Toward Oxidation
'
When Aroclor 1254 is heated for 50 or 60 days at 150C in the
presence of oxygen and copper, there is likely to be some attack on the copper. Examination of Aroclor 1254 after that period of time will usually show the presence of soluble copper. This also
occurs with mineral oil and other lnsulat ng liquids.
In general, even after severe oxidation conditions no evidence of chlorine splitting from the parent hydrocarbon has. been found.
Toward Acids ,
Aroclors 1242 and 1254 were stirred with an equal volume- of con
centrated Suirurlc Acid (96jS), dilute Sulfuric Acid (10J(), Nitric
Acid (70%), and dilute Nitric Acid (5%), at room temperature (25C)
for 150-250 hours. The Aroclor was then washed until neutral, de
hydrated with Sodium Sulfate, then analyzed in comparison with a
control sample for the various properties Which are regularly con
sidered, without causing these properties to depart from specifica
tion limits.
.
Aroclor 1262 was treated for 160 hours suspended in the same acids
as above at 50 to 55C. The concentrated Nitric Acid caused an inorease in color, otherwise no significant change in characteris tics.
The acid layer from the treatment of Aroclor 1254 was concentrated
Sulfuric Acid at room temperature for 150 hours and vas tested for
chloride content. The quantity of HC1 found was so small that it
was not possible by ordinary methods to obtain a quantitative fig
ure. Thus it appears that practically no hydrogen chloride is
evolved under these conditions.
-
HONS 092646
MONSANTO CHEMICAL COMPANY
10-1-44
COKROSIOil
Additional cirrosion data hot included in bulletin P-115 (PI 4-43-R)
la aa follows:
,><
Metal
Tamperature
. Tiara of Bxposure
Penetration ln/yr.
.
Monel Doe Metal
Telloe Braea
342C 150C
325C
A1 alloy 17ST 120OC A1 alloy 528H 120C A1 alloy 53ST 120C
360 hra. 40 daya
2,960 hra. in ateel bomb
21 21 21
.008 .001 ,003
.00035* .00035* .00038*
The weight loaa occurred in the flrat seven daya of
the test, negligible loss vas encountered in the last 14 daya.
The vapor condenser and the product receiver of the plant distilla
tion unit for producing Aroclor 1254 la constructed of Monel and no
failure in the system nor any noticeable reaction betveen the Aro-
olor and the Monel has been discovered after three years of opera
tion.
,
SOLUBILITY OF WATER IN AROCLOR 1242
The water content of a sample of Aroclor 1242 saturated with water
at approximately 30C was determined,using the Karl Plscher reagent,
to be about 0.080.
.............
Aroclor 1242, as regularly produced, contains by the same test less
than 0.0010 water, .
................
,.
SOBPACB TEWSIOH The surface tension of Aroclor 1254 is as follows:
'
Temperature
Dynes per Centimeter
25 C
80C
100C
.. . '
'
50.} 44.0
42.0
. .
Toxiom
:'
All chlorinated hydrocarbons have measurable degrees of toxicity,t the onisral organism. Ardclors are no exception. The symptoms of Aroolor poisoning are:' . .j sr*'
1. Pore acne (chlor-aehe)nodular eruptions ~bi' the hair follicles or sebaceous glands as a result of
....... insufficient cleansing of the skin'."~
.......... .
lisr-
MONSANTO CHEMICAL COMPANY
10-1-44
3. Acute yellow atrophy of the liver In wbleh the liver oelle show evening, hypergranulation, hyaline lneluelone and vecuolatlon ae a result of extensive, expo
sure over long periods of tlise.
These symptoms may aleo result frosi exposure to other chlorinated hydrocarbons of ooetneroe, such sat carbon tetrachloride, dlchlor-
ethylene, trlohlor ethylene, ohlorlnated naphthalene (Halowex).
The best knovn (at present) measure of the degree of toxicity of the Aroolors is presented below -
' Permissible Limits (in mg./cu.m.) of Concentration In Air of
Work toooma: (journal or Industrial Hygiene a Toxicology 3l:
I55.19J9)
~
Tested on Rats by Inhalation
Chlorine Content
___
Permissible
Limit mg./ou.m.
Aroolor 1368
` 68
Aroclor 4465
65
Aroolor 5460
60
Aroolor 1354
54
c Trlohlornaphthalene plus trace Tetrachlornaphthalene Tetra and Pentachlornaphthalenes
49.9 56.1
Penta and Hexaohlornaphthalenes
63.6
Tetra and Pentaohlornaphthalenes plus
Refined Chlorinated Diphenyl
45.5
900 Penta and Hexaohlornaphthalenes / 10J<
Aroolor 4465
65.0
Chlorinated Diphenyl Oxide
54.0
Chlorinated Diphenyl Oxide
57.0
Hexachlor Diphenyl Oxide / 5j< Trlohlor-
naphthalene
50-55
Hexachlornaphthalene and Crude Chlorinated
Diphenyl
.` '
Special Chlorinated Naphthalene
.
50-56
10.0 0.5 0.5 0.5
10.0 1.0 0.5 *
0.5 *
0.5 * 0.5 0.5
0-5
0.5 0.5
Tested also by feeding."
_.
Summary of Proas Feeding Experiments
Of the various materials fed rats in large doses, Trlohlornaphthalene
plus traces of Tetrachlornaphthalene was quite Innocuous. Tetra
and Pentaohlornaphthalene showed definite liver damage. Penta and
Hexaohlornophthalenes caused a similar grade of Injury. The addi
tion of chlorinated diphenyl to Penta and Hexaohlornaphthalenes
lnoreased the toxlelty. Chlorinated Diphenyl alone produced liver
l
lesions but In the dosage used vae leae effective than when'mixed . with highly chlorinated naphthalenes. In no ease" did the compounds '
;'&&&& . ... ...
HONS 09J64S
MORSAllTO CHEMICAL COMPARE
lO-l-^l if
cate this night he possible If one found a dosage vhloh could act
for the proper period of time.
' .;
Feodlng Precise Poses by Stomach Tube: The compounds employed sere suspended in gun hcaela. In figuring the dosage this total amount a nan of 50 kg. vould inhale In an 8-hour day, assuming on air con centration of 20 ngm. per cu.m., sas first calculated and reduced to milligrams per kilogram. Tbs rats and rabbits received this dose each day. Tho compounds ueed sere those employed ili the gross
feeding experiments and the results were essentially similar though the lesions sere less severe.
Subcutaneous Injections* 'The some gun acacia suspensions were ln-
jeoted suboufahoously Into rate end rabbits, the dosage being cal
culated on the basis of k ngm. per ou.m. of air. Again similar
results sere obtained. In all such experiments there must of nso- .
sssity be differences In the degree of effect but invariably the
liver sas the sole organ affeoted and the lesions sere those already
deserlbed many times.
:
Recommendations for Industrial Practice: Unless there Is a very
good reason for using the hot method o? Impregnation, all new' In stallations should use the cold or solvent method of impregnation with chlorinated naphthalenee and diphenyls. Where the hot method Is now being usod It should be changed over to cold, If possible, or surrounded with every known protective measure.
General hygienic measures should be followed, but In no ease should
these be allowed to supersede engineering control of the primary souroe of the exposure, the operations in the plant. '
The following hyglonio measures may be considered good practlee where these compounds are handledi
(a) Two lockers for each worker exposed to chlorinated saxes (one for working and one for street olothes).
(b) All work clothes above the underwear should be pro-
vlded and laundered .at,, least `twice a veek, by the .
management. . .
. '
'
'(o) The workers should change to clean underwear at tha and of each shift before getting into his street olothes.
(d) Supervised cleaning; (l) At noon the workers should
-
remove outer clothing and sorub hands and faoe under
supervision] (2) at the end of the shift they should
-
be required to take a supervised shover.before changing
.
back to treat Clothe*. .... *-
..
MONS 092649
KOlttAHTO CHEMICAL COMPANY
10-1-M
(e) Protective skin creams or protective clothing should be
provided by the management at the discretion of the fore man, nurse, medloal, or plant superintendent.
(f) All departments handling chlorinated synthetic vaxes
should be thoroughly cleaned according to a prearranged sohedule. This should include the removal of all de posits of waxy material from the maohines. floors and
surrounding objects. Workers doing the cleaning should be provided with protective clothing and supplied air or
organic vapor masks vhere exhaust ventilation is inade quate or not possible.
The foremen of all departments vhere this material is handled
should be apprised of the toxic nature of the material and in
structed in aafe handling procedures. These men should make it
their duty to cheok up on the workers In their departments and
Instruct them in safe practice.
'
Pre-employment and periodic physical examinations should be made
of all expoaed workers. These should include the taking of a full
clinical history, with special emphasis on gaetro-lntestinal dis
turbances and dermatitis. In addition, the skin should be care
fully examined periodically and the more reliable liver function
taste performed. Oastro-lntestinal complaints developing in a
vorker at any time should be a signal .for an immediate medical
oheok-up. A history of liver disease. Jaundice, or antlsyphllltic
treatment should automatically exolude a worker from Jobe involv
ing a possible toxic exposure. Pregnant women should not be em
ployed where there is a possible exposure to the synthetlo chlor
inated waxes,
.
Engineering control of plant operations oannot be over-emphasised
but specific recommendations are not applicable to all oases, it would be vise for a plant using this class of materials to check
their oontrol measures with the state industrial hygiene agency, the insurance carrier and Some competent consultant before occu pational disease' oooura........................
APPLICATIONS OP AR0CL0R3
AbHBSlVBS
Adhesives of good, electrical characteristics oan be prepared con taining Aroolors. The following are typioal examples:
#103 Aroelo* 4465 (Code 3140-0144)
(XV) Paraffin 50.600
...-
Mineral Oil (Ext(pa Heavy White)
Barytes - Met>ham*s #2
-
Typical Values
MONSANTO CHEMICAL COMPANY
10-1 -**
( Typical Values
#103B Aroclor 2565 (S.P. 77.5C) (Code 31*0-011*) (XB) Paraffin 50.8C
Mineral Oil (Extra Heavy White - Sonneborn 'e)
Barytes - Mepham's #2
*6.50#
1.17 8.33 50.00
#131 B-ll 65B
Aroclor **65 (Code 31*0-01**) Ester Oum - BKEO #1202XXXX Pale Paraffin 50.8C
Barytes - Nephan's #2
16.10#
14.35 *.55
. 65.00
oco
CUr-S
#135 Aroclor **65 (Cods 31*0-01**) Ester OUm - EK20 #1202XXXX Pale Mineral Oil '(Extra Heavy White - Sonneborn'e)
Barytes - Mepham's #2
5.85 55.00
#H Aroolor **65 (Code 31*0-01**)
50B Mineral Oil (Extra Heavy White - Sonneborn's) Barytes - Mepham's #2
*6.0#
*.0 50.0
#"M" Aroclor **65 Mineral Oil (Extra Heavy White - Sonneborn'e)
#"M" Aroclor **65 Mineral Oil (Extra Heavy White - Sonneborn's) Silica (Schulte, Champlain & Blbbo)
89.5# 10.5 .
50-8# 6.8
35-0
For the preparation of thermo-plastlo adhesives Purdue University found that the harder Aroolors are better than anything else dis
covered to date, primarily because of their high compatibility with other resins and their thermo-stability.
ELECTRICAL
Dielectrics and Kleotrloal Insulators
The Aroclors have excellent dielectric properties, that is, low
dlelectrio constant and resistivity and low power factor. Aro-
clor 12*2 has the highest dielectric constant of the whole series
which we are manufacturing commercially, while higher chlorine
Aroolors have higher resistivity.
The Aroclors have found usefulness as a dielectric In condensers and as a dlelectrio and cooling medium In transformersi and a
number of miscellaneous similar uses where the characteristics above named are of Importance.
AROCLORS AS SATURANTS
Saturation may be defined as that operation by which liquids or gases ore caused to penetrate relatively parous materials. The penetrating medium Is known as the saturant and is generally In
N0H3AMT0 CHEMICAL COMPANY
10-1-4%
the liquid state. Saturation nay be assisted or aocelerated by means of increased temperature and pressure or by the use of a
vacuum.
Various dosses of products are saturated for the purpose of giv
ing them a vide variety of properties. Sane of the properties
attained by saturation are: water' and flame resistance; resistance
to chemicals; abrasion; moisture; light and weather changes; in
creased strength; and increased weight.
,,
;.
Among the articles that are treated to obtain some one or all of the above mentioned properties are included the various fibres and
fabrics: animal; vegetable and mineral; woods, both hard and soft; c'eramios ware and cement; and certain kinds of electrical appara
tus, such as oarbon resistors.
The saturants', or, as they are sometimes called, the lmpregnants,
are usually made up of waxes, oils, resins, or water solutions of
oortaln Inorganic salts.
.
Applications
At present the saturating applications that are of chief interest are Insulated wire, low voltage oable commonly called network cable, and oarbon resistor fields. These proposed uses are des cribed more fully under the separate headings which follow.
network Cable
1
Attempts are being made to develop a use for Aroclor as-a saturant
for secondary network or lpv voltage cable. . Cable of this kind Is
used in electrical network distribution systems. Oenerally, It
consists of the copper conductor or conductors, the paper insula
tion, and the lead sheath. The paper is saturated with an oil.,
usually a good grade of oil such as the General Eleotrlc Company's
Trans11 Oil. This fora of construction Is objectionable because
under the conditions Imposed by a short circuit, combustible gases
are generated which flow through the conduits to the manholes, at
which point they may form explosive mixtures with the air and. In
turn, cause explosions in the manholes. Both the paper and the oil
are source# of eombustible gases. It Is therefore desirable to
replace them -- the paper with an Inert form of Insulation, If
possible, and the oil with a non-inflammable saturant such as Aro
clor. Thus far, Aroclor 123% appears to meet the requirements of
this use.
.
The more important cable manufacturers In the country are already at vork on the development of a flame resistant cable and also one In vhloh the explosion hazard will be lessened or eliminated.
Monsanto chemical company
10-1-4%
Carbon Resistors
-
Carbon realatora are email molded rode of a mixture of oarbon blaok and Band with a realnoua binder. They are porous and their elec trical roelstance la seriously afrected by the entrance of molature.
To prevont molature getting Into the unite they are usually impreg nated vlth'some, material to fill up the voids and to coat the sur
face of the resistor. A vax le generally used for this purpose and serves very veil as far as moisture-proofing Is concerned. Hovevor, after completion, the resistor must be lacquered for Identi fication. Lacquer does not adhere veil to the vaxed surfaces.
Aroclor 4465 Moisture-proofing Compounds give moisture proofness
(Humidity test) equal to that of vax and, In addition, give a sur
face to vhloh lacquer vlll adhere.
.
The Aroclor Compound Is non-cryatalllne and therefore does not have
a definite melting point and does not become extremely fluid at the melting point of most vaxes that are used In this application, but it gradually softens under Increased temperature.
In extensive teats to find the moat effective medium for Impregna ting radio resistors to stabilise the electrical resistivity undvr exaggerated and extreme humidity tests, Aroolor 5460 gave by far the best results vhen compared vlth Santovax and various petroleum
vaxes and compounds.
This excellent Aroclor success vas accomplished by grinding off or sanding the surface of the carbon resistor prior to Impregnating,
thus exposing the Inner pores of the resistor, permitting excellent penetration. Penetration has alvays been a problem In the Impreg nation of resistors vlth resinous materials suoh as Aroclor.
Cable Insulation
'
Electrical conduitore and cables Insulated vlth asbestos are fre quently lacking In vaterproofness. Impregnation vlth vox canpoei-
tions gives an Insulating medium resistant to atmospheric moisture and sometimes even to Immersion In vater for a short time, but
hitherto no composition having the required characteristics of heat resistance and flameproofness has given sufficient voter re sistance to withstand Immersion for prolonged perlode.
An Improved method of Impregnating asbestos Is described in tJ. 3. Patent 2,162,953, assigned toRockbestoe Products Corporation, vhlch depends on the use of a phenolic resin In conjunction vlth . a chlorinated diphenyl. Xt has already been proposed to use each of these substances separately for a similar purpose, but alone
the first lacks flameproofness and the second resistance to water.'
.Si--
MONS 092653
MONSANTO CHEMICAL COMPANY
10-1-M
The phenolic reeln used for this purpose should be thermoplastic, solid and rather brittle at ordinary temperatures, with a flow ' point of 105C. Bakelite XR 8430 Is suggested as a suitable type. The best chlorinated diphenyl for this process is stated to be one having a viscosity of 9 see* Saybolt at 100Ct and, of course. It must mix readily with the phenolic resin. One containing about 62 per oent chlorine Is said to be satisfactory, for example, Arc elor 1262.
The two Ingredients are mixed In equal parts by weight at 166C, preferably with the addition of 5 per cent by weight of a plastiolzer such as Trlcresyl Phosphate. The resulting mixture Is stable and oan be stored.
In manufacturing the cable the individual conductors are Insulated,
twisted and covered with the layers of Impregnated asbestos and varnished cambric (or the like) In the manner well understood In the art. A layer of loosely felted dry asbestos of suitable thick
ness Is then applied around the thus assembled cable, and a dry asbestos braid Is applied over the felted layer of asbestos. The so-oovered cable Is then passed through the Impregnating compound (mixture of resinous phenollo condensation product and chlorinated diphenyl) while maintaining the compound at a temperature of about
155C. The time required to Impregnate the layer of felted asbes tos and asbestos braid will depend on the thickness of the layer.
As the cable emerges from the heated bath of Impregnating, compound,
It Is passed through suitable snubbing devices to remove the excess compound from Its outer surface.
In order to prevent migration af the outer surface compound when
the finished wire or cable Is subjected to high temperatures In service, It has been found advantageous In sens Instances to ap ply to the Impregnated layer of asbestos a second coat of the
Impregnating compound to which has been added about 15 to 20J< of ground mica or other finely divided Inert solid material. The Impregnating compound on the outer surface of the impregnated asbestos then contains dispersed finely divided particles of the
Inert solid material which act to thicken the compound and render It less susceptible to flow. The admixture of mica or the like
Is not required or desirable In the compound used to Impregnate
the asbestos layer, since the asbestos fibres themselves satisfac torily perform the function of retaining the compound within the mass by capillary attraction.
The Insulated conductor or cable of the Invention poaaesses all the necessary characteristics of heat resistance, flameproofness, pliability, dielectric strength and resistance to water. The outer Insulating layer of asbestos Impregnated with a mixture of
resinous phenolic condensation product and chlorinated diphenyl Is substantially waterproof, even when submerged In Mter for ex
tended periods of time or subjected to hydrostatic pressure as ' high as 25 pounds per Square Inch. In general, the ue of asbestos
-12-
MQNS 092654
. . _______
10-1-44
r MONSANTO CHEMICAL COMPANY as an electrical insulating material has heretofore been limited to locations vhere high temperatures or the hasard of Inflammable
material made the use of ordinary forms of Insulation (such as rubber, varnished cambric, paper, etc.) undesirable or prohibitive. It'vlli, therefore, be evident that the invention widely extends the usefulness of asbestos Insulated wires and oables.
Condensers
.
A rapidly growing use of Aroclor Is In the manufacture of the small
condensers employed In fluorescent lighting fixtures for offices,
business houseB and factories. .
.
AROCLOR EMULSION FORMULA
16 pounds of Aroclor - liquid 8 pounds of Water
. 16 ounces of Stearic Acid 4 ounces of Triethanolamine
The Aroclor is heated to a workable viscosity above 82C (180F) and the Steario Acid Is added and completely stirred In. The water is heated to 97C (207F) and the Triethanolamine added and
c thoroughly stirred in. After both of these operations have been carried out, the Aroclor-Stearlo Acid combination is poured Into the voter mixture while the latter Is well agitated and then the whole mixture lp processed through a colloid mill. Good results may even be obtained without the use of a colloid mill, provided the mixture Is agitated with a high-speed emulsifying stirrer.
FLAMEPR00FER5
.
The Aroclors are not Inflammable and when mixed in sufficiently
large proportion vlth many other materials have rendered the can-
pie te compound non-inflammable. For Instance, a mixture of about
equal parts of Aroclor 2565 and aaphalt gives a resulting compound
that will not permit the spread of flame. Wood may be Impregnated
sufficiently with one of the higher chlorine Aroclors, such as
4465, that It will pass the most rigid tests now applied to wood
which has been treated for flameproofness, such as the tests used
by the Forest Products Laboratory and by the Building Department
of the City of New Tort.
..
We have not yet found a market for Aroclor in the field of flame
proofing wood because In most cases vhere the wood Is treated for flameproofness It Is used Indoors where It Is not exposed to
leaching by rain, so that one of the phosphate salts Is generally used, However, there may be special uses where these materials are not acceptable ap{d where the prlos of Aroclor is justified.'
( :
''
10-1-44
( M0K3ANT0 CHEMICAL COMPANY
There la throughout the country a tremendous market for compounded waxes for all manner of uses. It la very likely that In some of the applications of these materials it would be desirable to havf them non-inflammable. It Is also likely that the incorporation of Aroclor with some other resinous or waxy materials would give other desirable properties. These applications oould probably be worked out In conjunction with companies who are now in the business of , compounding and selling such materials. There are some of these companies In each of our sales territories. ,
Aroolors 4465 and 5460 are the most likely ones In this application.
Tests are under way to determine the suitability of the substitu tion of Aroclor 1260 for chlorinated paraffin In the treatment of paullns and tentage for use by the Army. This Is for the purpose of producing non-lnflaipmability, Improving moisture resistance, and mildew proofing.
The Aroclors are remarkably stable and their superiority in this
respeot to chlorinated paraffin customarily employed for this pur
pose le demonstrated In the following results reported by our
laboratory.
.
-
c Light Stability Tests In order to be certain that the tests were comparable In every respect, they were conducted by personnel of the A. French Textile School, Oeorgla School of Technology, Atlanta, Oeorgla.
The samples used in these tests had been prepared at Anniston prior
to this visit. They consisted of sections of klerbolled ootton
sheeting Impregnated with compositions as shown In the tabulation
below. Approximately 10{f of chlorinated hydrocarbon vas applied to each of the Impregnated samples. The chlorinated paraffin used had the following characteristics: -
* C12 Sp.Or.
e
. 25/25C
43.15 1.183
Viscosity 210op I75 3U3
Pour Point
-8P
As will be noted, several pigments, namely, P2O3, BbgO^, and
CaCOx, were also applied to the fabric. These pigments were used In tne following proportions:
FegOj - 10 parts PegOj to 8 parts chlorine In the chlor inated hydrocarbon.
.
Sb20j - 10 parts Sb^Oj to 8' parts chlorine, ( CaC03 - 7i parts CaCOj to 10 parts chiorlns.
MONSANTO CHEMICAL COMPANY
10-1-**
In the testa with the pigmented mixtures, the pigment adhered to the surface of the cloth and was not very evenly distributed.
The actual tests made at Oeorgia Tech. Involved exposure for two hours In a Cooper-Hevett lamp cabinet, thon conditioning at 70F
and 65Jt H.H. for four hours or longer, and finally testli^ for varpwlse tensile strength by the grab method with a Scott tester. The Cooper-Hevett cabinet had a Uviare (fused quarts mercury arc)
lamp aa the aouroe of ultra-violet light. On the basis of dye fading testa conducted at Oeorgia Tech, over an extensive period several years ago, two hours' exposure In the Cooper-Hevett cabinet
Is roughly equivalent to 20 days' average outdoor weathering. This relation does not necessarily apply to tensile strength deteriora tion tests. Judging by the deterioration of the tensile strength of unimpregnated samples, it would appear that 2 hours' exposure In the Cooper-Hevett vas equivalent to much more than SO days' out side exposure.
Summarised data for the tensile strength tests were as shown In the
following tabulation:
,
Impregnation Mixture
Tensile Strength (X)
Unexposed
Exposed
Wo.no (Plain doth only)
Chlorinated Paraffin M II ft Pe203 ft 3b203
ft CaC03
Aroclor 1254
ft Pe203
ft 3b203 ft CaC03
Aroolor 1260
ft Fe203
ft Sb203 ft CaC03
.
55-75
57.75 60.9 57.0 57.9
5*.5 60.1 56.2 53.75
59-^ 58.0 62.4 59.25
27-9
13.1 17 75 '17.5 18. 5
2*. 0 27.1 ' 2*.5 25.9
25.75 30.1 3*.9 30.9
Arodor 54*2
II H
ft Pe203
ft Sb203 w
ft CaC03
60.1
65.5 63.9 62.*
33.5 . 3*.l
*0.6
*0.9
(X) Units aro in-pounds and, except for three Instances, the
values shown are averages of * tests, -
S ' , ,,.
. . *iT-
'
The conclusion from these tests vas that the Aroclora contributed
little, if any, to the deterioration of tensile strength of the doth upon exposure to ultra-violet light, whereas chlorinated paraffin did appreciably accelerate deterioration under the same
........v... .
i
HONS 092657
10-1-44
MONSANTO CHEMICAL COMPACT
r
conditions. Also, under the conditions of these tests, all of the pigments tried decreased to some extent the tendering effect of the ultra-violet light. This is probably not abnormal, sinee the pigments should have reflected a portion of the light rays.
It has been reported that certain pigments decrease the heat sta bility of ohlorlnated paraffin, thus accelerating tendering of treated cotton goods upon exposure in hot climates. Beat stabil ity tests on all of the impregnation mixtures tried as outlined above are nov being run in the laboratory at Anniston.
Compared vith plain cloth unexposed (100$) the hydrocarbon treat ments alone effected the folloving Improvement In tensile strengths
Chlorinated Paraffin Aroclor 1254 Aroclor 1260
Aroclor 5442
7.5^ . 1.3*
10.55<
11.8#
This increase in tensile strength through impregnation is compen sated for in the folloving calculation.
When the "Exposed Tensile Strength" is expressed as per cent of "Unexposed Tensile^ Strength" the folloving relationship is evident:
Untreated Cloth
Per cent Resistance to Deterioration on Exposure - to Ultra-violet Light
51.9
Chlorinated Paraffin n ft Fe203 ft Sb203 it k CaC03
Aroclor 1254 II II It n It
k Fa203 k Sb203 ' k CaC03
Aroclor 1260 II II II
k Fe203 4c Sb203 ft CaC03
Aroclor 5442
ft Fe203
ft SbS03 ft CaC03
*
28.10 29.15 31.40 31.52
44.05 45.10 43.62 44.19
43.36 51.86 56.00 52-10
55-70 52.05 63.53 65-53
' . *
(
The advantage of the Aroclors in comparison vith Chlorinated Par affin as a non-inflammable, waterproof lmpregnant for cotton fab
ric as measured by resistance to loss of tensile strength on ,
-16-'
MOMS 092658
/r.-'.r:
MOHSAUTO CHEMICAL COMPAHY
10-1 *4
exposure to ultra-violet light Is expressed In the following re lationship, basis equivalent Chlorinated Paraffin treatment as
100*;
Per cent Improvement In Resistance to Deterioration
over Comparable Treatment
with Chlorinated Paraffin
Aroclor 1254 * Fe203
ft Sb203 k CoC03
Average
56.7 54.7 42.1
40.1
48.4
Aroclor 1260 k Pe203 ft Sb203 ft CaC03
Aroclor 5442 ft Fe203 ft Sb203 ft CaC03
Average Average
54.3 77.9 78.3 65-3
98.2 78.6 102.2 107-9
68.9 96.7
Heat Stability Tests
,
These tests were made by absorbing and titrating the HC1 evolved from 20 grams of chlorinated hydrocarbon when held at 175C and
blown with air at the rate of 0.01 cubic foot per minute for four hours. This Is the method outlined on pages 375-378 of the Aug ust 30, 1943, Issue of the Amerloan Dyestuff Reporter, Vol. 32, Ho. 18. James R. Redmond, Textile Technologist, Jeffersonville, Q.M. Depot, was the author of the article.
Data for the tests that have been completed were as follows:
Chlorinated Hydrocarbon Composition
% HC1 Evolved In 4 hrs at I75c
20 amis. Chlorinated Pararrm
20 gms.
"
" f. 2.0 gms, Fe203
20 gms.
*
* f 10.5 gms. Sb203
20 gms.
"
/ 6.3 gms. CaC03
20
20 20 20
gms.
gms. gms. gms.
Aroclor
" " "
12(1 54
ft tt
f. 2 gms. Fe203
2 gms. Sb203 / 2 gms. 0aC03
0.4l 20.00
0.29 .0.29
0.00 0.01 . 0.01 : . 0.02
HONS 091459
10-1-44 ( MONSANTO CHEMICAL COMPANY
Chlorinated Hydrocarbon Composition______________
# HCI Evolved In 4 hrs, at 175C
20 20 20
gms. gms.
gms.
Aronelor tt
12n 60 ti
20 gras.
M
it
A ? gms. Pe203 / 2 gms. 3b203 A 2 gms. CaC03
.
0.002 0.02 0.005 0.01
20 20
20 20
gms. gms.
gms. gms.
AroIeI lor
ft ft
5t^i 2 rr M
/ 2 gms. 7e203
A. 2 gms. Sb203 A 2 gms. CaC03
, 0.00
0.00 0.02 0.02
These data clearly demonstrate the markedly superior heat stability of the Aroolors as oompared to chlorinated paraffin. Particularly
significant Is the accelerating action of Fe203 on the decomposition rate of chlorinated paraffin. No such accelerating action was noted
with the Aroclors.
While in most of the testa with the Aroclors our titrations Indi
cated the evolution of HCI ranging up to 0.02$, the titrations were
so small as to possibly be within the range of experimental error.
At any rate, we are quite sure that 0.02# HCI evolution represents
the maximum HCI loss under the conditions of the tests.
( Chlorinated Hydrocarbon
% HCI Evolved In
Mixture ______________
4 hrs, at 175C
20 gms. Chlorinated Paraffin and 2 gms. Zinc Borate #316?
20 gms. Aroolor 1254 and 2 gms. Zinc Borate #3167
12 gms. Aroolor 5442 and 8 gms. Tricresyl Phosphate
12 gms. Aroelor 5442 and 8 gms. Tricresyl Phosphate and 2 gms. 7e203
12 gms. Aroolor 5442 and 8 gms. Tricresyl Phosphate and 2 gms. 3b203
12 gms. Aroolor 5442 and 8 gms. Tricresyl'Phosphate and 2 gms. CaC03
12 gms. Aroelor 5442 and 8 gms. Tricresyl Phosphate and 2 gms. Zinc Borate #3167
.
' '
>
15.6 0.01 0.02 0.00 0.01 0.00 0.01
Again it will be noted that the Aroclors are far more stable than Chlorinated Paraffin lh the presence of Zinc Borate,
MONS
; -10-
MJ.r'~i
*
xr.-.v-' .;..:..V.,
092660
10-1-** ^ MONSANTO CHEMICAL COMPANY
HEAT TRANSFER MEDIUM
Aroolor ha# been used for a number of years at Anniston as a heat transfer medium. It Is now employed as such In the HB-*0 plant.
Company (075050) used Aroclor as a heat transfer modiurn in maln-
tainlng a molten lead bath In vhleh they soaked 1* Inch armour
plorolng projectiles. They operated one unit using Aroolor and
another using Dowtherm. Both of these units were used for several
' years. They then discontinued the use of Aroolor after dlscover-
lng corrosion In the Aroclor system, which did not occur in the
Dowtherm system.
,
A company developed some equipment for heating pyrites In which they Intended using Aroclor as the heat transfer medium. Since
the equipment was never sold commercially, none of these units involving Aroclor are now In operation
Many people considering Aroclor as a heat transfer medium gave It up either becauae it would not stand the temperature they required,
or on account of fumes coming from the Aroclor, or because It cost more than oil normally used for this purpose.
Favorable features to the use of Aroclor for this purpose are:
1. Liquid at room temperature.
2. Does not oxidize.
3. Has nearly twice the speciflo heat of petroleum oils generally used for this purpose.
'
4. Non-Inflammable.
HYDRAULIC FLUID
Company (576,450) operating a high pressure steam-electric gener
ating plant use Aroclor 1248 as an hydraulic medium In their gov
ernor system. They do not use It as h lubricant. The Aroclor Is
used instead of oil, merely because of its non-inflammability.
When oil Is used In the governor system. It la customary to use the
same oil reservoir, both for the lubricating and governor systems.
When Aroclor Is used In the governor system and petroleum oil In
the lubricating system, it Is necessary to segregate the two sys
tems and use separate pumps for the lubrloatlng and governor sys
tems .
,
Westlnghouse have been the principal promoters of the use of Aro
olor in the governor system as a result of having the oil In a
( governor system catoh fire In one of the Jefreoy Central Light and
Fower Company's stations while Westlnghouse engineers were working
with the unit.
........,,... .
,
.,
' ..
HONS 092661
10-1-44 MONSANTO CHEMICAL COMPANY (
ENAMELS
Company (104460) has obtained some Intereating reaulta with bakedon enamels containing Aroclor 125*1, Acrylold Resin and Trlcresyl Phosphate, pigmented with Titanium Dioxide and Zinc Oxide. The
enamel is baked on at 135C (275?)- They have found that Trloresyl Phosphate aids the Aroclor on baking, giving a hard surface.
This same company has found that mixes of Aroclor and Vlstanex
(No. 6 B-80 and B-100) or Aroclor and Vlxtac (No. 1 and No. 2)
glvo Interesting properties somewhat like shellac. They state
that these produots have good adhesion.
.
LACQUERS
We have a very good general line-up on the use of Aroclor In lao-
quers In the booklet P-115 which ve have published for distribu tion. This booklet gives the limits of compatibility of Aroclors 1254 and 1262 in Nitrocellulose lacquers. Since this booklet has boon published, a number of companies have started using Aroclor 1242 In special flexible lacquers, such as are used on high ten sion cables, etc. The compatibility limits of Aroclor 1242 are
higher than those of the higher ohlorlne Aroclors so that It Is possible to Incorporate enough of the Aroclor to give It extreme
flexibility. You have the formula for Aroclor Lacquer No. 34
which glvos the details of the use of this Aroclor in cable lac quer.
The work done In our laboratory using Aroclor In lacquers Indi cates that we get somewhat less chalking with the Aroclor lacquers
than with those made up by other formulae. We get practical free dom from checking and cracking and, we believe, better color re tention In the vhite and light colored lacquers. These are Impor
tant considerations In lacquer manufacture, and Aroclor should be given muoh more consideration from now on for general use such as an automobile lacquer, etc., than It has received In the past because of the rising prices of other resins which are generally used.
We have a number of customers who use Aroclors 1242, 1254 and 1262 In the manufacture of lacquer.
Lacquer Formulation Chart
Non-Volatile Constituents
1. A resin
2. Nitrocellulose (cellulose nitrate)
3. A plasticiser or softener
-
i" '...... -20 ' .........
't
092462
MONSANTO CHEMICAL COMPANY
10-1-**
Volatile Constituents
'
1. The alcohol constituent 2. The ester constituent
3. The hydrocarbon constituent
Finished Lacquer
.'
X per cent of the non-volatile (100 - X) per cent of the volatile
.
The percentage X, of the non-volatile or film-forming constituents, may vary betvoen 20# and 30# of the veight of the finished lacquer
Non-Volatile Constituents
.
As has been shown by the table, the non-volatile components of a
lacquer consist of a resin, cellulose nitrate and a plasticiser or softener. For the rosin, some one of those of synthetic origin
may be employed, or a natural resin such as Gum Dammar may be used. Oum Dammar Is a generally used resin in lacquer formulation, and It
can be taken as the number one component. The number two component is the cellulose nitrate Itself. It is also lenovn as Nitrocellu lose, Pyroxylin and "PX." To the Industry in general It is "cotton.1 It can be purchased in two kinds, the AS and RS grades. The latter grade Is the one that Is chiefly used by lacquer manufacturers.
The initials Indicate a difference In the method of manufacture,
AS meaning that the cotton Is alcohol-soluble, and RS meaning that
it Is regularly soluble.
..
Both grades are usually bought wet with denatured alcohol. The
viscosity of the cotton is another detenslnlng factor with regard
to Its use. The cotton that.is commonly employed by the Industry
has a viscosity of one-half second and la known as "half-second
cotton." For the third component dibutyl phthalate, trloresyl
phosphate or castor oil may be used.
.
At this point an explanation of the terms "plasticiser" and "sof tener" becomes necessary. The average lacquer technologist uses
these terms synonymously, and for this reason they have come to mean almost one and the same thing in this Industry. Strictly speaking, a true plasticiser should be a solvent for tbe "cotton"
and the resin. In addition. It should have a lov vaporisation
loss and should confer such properties as flexibility, pliability, and durability on the lacquer film. Both dibutyl phthalate and
trlcresyl phosphate meet these requirement*, Castor oil, on the other hand, does not. In that It Is only a partial solvent for "cotton." It does, however,1 give to the film the qualities al ready mentioned, In short. It exerts a softening effect - hence
the name "softener." The difference,'then, between a plasticiser and a "softener" is that the former ia,a true,solvent,for the
HONS 092663
, ' 1Q-1-M
" MORSAUTO CHEMICAL COMPARE
non-volatile constituents of a lacquer, vhlle the latter Is a non
solvent, or, at best, only a partial solvent. Castor oil is typi cal of this latter class and is widely used as a lacquer "softener."
Volatile Constituents
The volatile constituents fora what la known as a balanced solvent
mixture, the purpose of which is to be used as a solvent or thinner for the non-volatile constituents. The components of this mixture
must be in such a proportion to each other so as to Insure a uni
form evaporation rate when the lacquer film dries, and also to make sure that no precipitation of the "cotton" will occur at the time
of thinning.
The number one, or the alcohol, component is generally composed of ethyl alcohol - 95$ and butyl alcohol. The ester component is made
up In general of ethyl acetate and butyl acetate, vhlle the hydro carbon component usually consists of some compound such as toluol
or, for special lacquers such, as cable dopes, benzol.
Finished Lacquer
The finished lacquer Is prepared by taking a given weight of the non-volatile constituents and dissolving them in a given weight ci the volatile constituents.
Competition
The question of competition will have to be viewed from two angles;
first with regard to the Aroolors as resins, and second with regrr.l to them as softeners. Since the Aroolors have more the properties
of softeners than of resins, the softeners are nearly competitive with the Aroclors than are the resins.
Competing Basins - Synthetlo
Name
Number
Manufacturer
Amberol
801 The Beslnoue Products & Chemicals Cc.
Philadelphia, Pennsylvania
'
Bakellte
XB-502
Bakellte Corporation New York, New York
-.
.
Beckaolte
(iu)
law)
Beck, Roller it Company, Inc.
Detroit, Michigan
.
Olyptal
1202'
General Electric Company Schenectady, New York
Levied
If!...
John D. Lewis, Inc. ;; Providence, Rhode Island
'
'
\%'A,
V`
. -22-
> hONS 092bb<'
. , . ....
n
..
MONSANTO CHEMICAL COMPANY
10-1-44
Competing Regina - Synthetic
Name
Number
Manufacturer
Paraplex*
The Resinous Products & Chemicals Oo. Philadelphia, Pennsylvania
Rezyl
(ill
American Cyanamld & Chemical Corp. New York, New York
Rezyl Balsams -
American Cyanamld & Chemical Corp. New York, New York
Teglacs
-
American Cyanamld & Chemical Corp. New York, New York
Paraplex can probably be considered a softener as well as a resin.
Competing Resins - Semi-Synthetic
Name
Number
Manufacturer
-
Ester Oum
None
(One of the most
generally
used resins.)
There are many manufacturers
Natural Regins
Oum Dammar
(Batavia) (Singapore)
Imported - obtained through brokers
Competing Plasticizers or Softeners
Name'OradeTrade NameManufacturer
Dibutyl Phthalate* -
Monsanto Chemical Co. St. Louis, Missouri
Trlcresyl Phosphate* -
Monsanto Chemical Co. St. Louis, Missouri
Kronltex Kavalco Products, Inc. Nltro, West Virginia
'
Llndol
' Celluloid Corporation
Newark, Nev Jersey
Abalyn
, '
(A rosin product
recommended for lacquer formulation)
Hercules Povder Company
Wilmington, Delaware '
-23-' - ; -'V'-
MONS 092665
10-1-44
MOHSANTO CHEMICAL COMPANY
( Competing Plasticizers or Softeners
NameQradeTrade MaineManufacturer
ABM-100
(A modified linseed oil for lacquer formulation)
Archer-Daniels Midland Ccx Milwaukee, Wisconsin
Castor Oil (Baker's)*
Number 4 Rumber 15 Humber 10
AA
Blown The Baker Castor Oil Co.
Blown Jersey City Mew Jersey Blown Unblown
Spencer-Kellogg Oil
(A modified castor Spencer-Kellogg A Sons
oil for lacquer Buffalo, New York
formulation)
'
Vhere are other manufacturers of these products - this list Is by no means complete.
In listing these products, only those that are In more or less gen eral use have been Included. There are some notable exceptions,
however, In the cases of such materials as Abalyn, ADM-100 Oil, and Spencer-Kellogg Oil.
i The materials listed In these tables must not be thought of en
tirely as competing products because they may be more Important
as aids or auxiliaries In co-development work with the Arodlors. In fact, It Is believed preferable to regard them more In thle light than as competitors.
Advantages
In thinking of any advantages the Aroclore may have, the statements
made In the final paragraph under "Competition" must be borne in mind. It Is preferable to confine oneself to a discussion or the
outstanding properties of the Aroclore, for It le believed that It Is only through the development of some specific property that progress is going to be made.
The properties of the Aroclors thot should be emphasised are:
1. Low vaporization loss
2. Pale oolor . . '
5. Adhesion 4. Chemical Stability
a. , to light
b. to water, aclde and alkalies
c. to heat
(
d. to oxidation a. to chemical action In general
hONS 092666
-24
MONSANTO CHEMICAL COMPANY
10-1-44
5. Non-Inflammability
6. Non-corroelvenesa 7. Solubility in commonly Used looquep solvents
A resume of the properties that Aroclors impart to lacquers and
the types of lacquers for vhlch they are recommended may be given
briefly as follows:
'
In a Dammar-type laoquer the plasticiser-softener combination, such os the usual dlbutyl phthalate-costor oil combination, may
be advantageously replaced by an Aroclor alone. Tho resulting
lacquer is less subject to checking and cracking on outside ex posure and retains its gloss. i
Aroclor 1262 may also be substituted entirely for the resin in certain types of lacquer. The clear lacquer, so produced, is practically colorless and provides an excellent base for white enamels. Such enamels, however, do not withstand weathering as well as those containing Dammar in addition to the Aroclor.
The advantageous properties of the Aroclors in Imparting added
weather resistance to properly formulated lacquers may be traced
to their resistance to the action of sunlight, to their perman
ency in the film, and to their extreme ehemioal stability. The
Aroclors do hot oxidise, "dry," or harden. The Aroclors are un
affected by dilute adds'and even by hot oauetic solutions. They
are not subject to polymerisation, rancidity on* other change, as
far as is known.
',
When added to a nitrocellulose solution, the Aroclors reduce the vlsoosity slightly. This change in viscosity takes place at once
and no further change due to the presence of the Aroclor occurs on several months' aging in closed containers.
By virtue of their high refractive index, they impart apparent
depth to the lacquer film. Aroclor 1262 has adhesive properties
and the lacquers containing it have good adhesion. Lacquers con
taining the Aroclors dry normally and give a hard, non-tacky,
durable film of excellent gloss-
_
Certain laoquer technologists have found that a lacquer contaifi^g
Aroclor can be polished with a minimum of rubbing and, furthermore,
that the Aroclor seems to Impart a harder finish to a lacquer film
than oils, trlcresyl phosphate, or dlbutyl phthalate. It has also
been reported that properly formulated lacquers containing Aroclor
show no tendency to "spew" or "sweat out" when buffed.
-
In addition to the properties of general interest,: other proper ties of tho Arocloro arc of V-.lue in formulating lacquers to fit
special requirements. Arocloro 1254, 4465, 5460 and 1262 do not support oorabustion, and when present in nitrocellulose films they
> -25-
mons 092C<>7
MO1AUTO CHEMICAL COMPANY
10-1-44
,
retard the rate of burning. The Aroclore retard the rate of trans
fer of moisture and of gases through a nitrocellulose film, and by virtue of this fact have already found extensive use In protective lacquers for application over those types of electrical Insulating materials, such as rubber, that deteriorate rapidly In contaot . vlth oxygen, 02one, moisture or other vapors.
Procedure
'
Upon visiting a lacquer company, every effort should be made to ,
see the chemist In oharge of formulation or production. In large
companies the director of research should always be seen. As a
general rule, a great deal will not be accomplished until these '
respective individuals are seen.
.
[
A complete discussion of the properties of the Aroclors should be
given, emphasis being plaoed upon the possible formulation of a new lacquer vlth some one of these properties ae the background.
When discussing the use of Aroclore In lacquers, the salesman Bhould remember that the Aroclore are not solvents for nitrocel
lulose and that for this reason an excessive amount of Aroclor must never be used In the formulation of a lacquer.. The limiting percentages that can be used for successful results have been
carefully worked out by a large number of experiments. The few simple rules that must be followed In formulating lacquers with
ths Aroclors are emBoJled In a booklet entitled "The Properties
of Two Aroclors of Special Interest to Manufacturers of Lacquers." Copies of this booklet may be had on application to our sales
offices. It Is recommended that the salesman offer copies of thJ s booklet and the bulletin "Plasticisers A Resins - Organlo Division"
to Interested lacquer manufacturers.
Attempts should be made to determine what particular lacquers a
manufacturer specializes In and what problems he is studying at
tbe time of the coll.
.
Aroolors have fair or good compatibility with nitrocellulose, Forravar, Butvar, vinyl copolymers, polyvinyl acetate, poly-etyrene, chlorinated rubber and ethyl cellulose. In general, the liquid or
semi-solid Aroclors act like true resins. One principal value la their chemical Inertness. Where great flexibility IS to be ob tained, it may be necessary to employ auxiliary plasticizers.
3onu of the exceptions are In chlorinated rubber and in ethyl
celiuloee where flexibility or hardness may be varied simply by selecting an Aroclor of the proper physical characteristics.
The liquid Aroolors such as 1242, 1248 or 1254 will greatly In crease flexibility but will cause softness. . The semi-solids such as 1260 or 5442 will Impart seme flexibility Without the marked softening effect. The brittle, resinous Aroolors such as 4465 or
5460 produce very hard compositions vlth excellent adhesion and
-26-
MUNS 092668
T
' MONSANTO CHEMICAL COMPANY
10^1-44
weathering qualities. If a single Aroelor does not impart the de
sired combination of properties, usually some mixture of Arociors
will do so. It vould seem that in polystyrene molding composl,
tlona, the resinous Arociors could be used as a flux or flow pro
moter at molding temperatures without causing softness and flow, at
normal temperatures. Some mixture of Arodors or a combination'
of an Aroolor with another plasticiser either solid or liquid ;
might be required for this purpose.
'
Of course, it is well known that for alkali resistant coatings, .
combinations of Aroolore (1254-1260 and 546o) with chlorinated rubber have been used for a long time. At the present time, the
use of equal parts of Aroelor 5460 and ethyl cellulose is being
pushed by Company (331850) as a weather resistant coating. Sim ilar coatings of low vleooslty polystyrene and Aroclors would
probably be of value.
ARMY-NAVY AERONAUTICAL SPECIFICATION
LACQUER - CAMOUFLAGE
AN-L-21 8 October 1943 - Page 14
TABLE IV
Control Formula - Clear Vehicle
Weight
Weight
lbs. per
Ingredients
Percent 100 gal.
Paraplex RO-2
(100*) 11.1
90
Amberlac B-94
(80* in xylene ) 5,6
45
Volume gal.per 100 gal.
.
'm
Arcelor 5460
(100*) 4.3
33
.
Ethyl Cellulose (3 to 4 sec)(100*1 ,,Cellulose-Nltrate/(g1c/4g slheee.Rth.Sy.l)'
' alcohol)
4.3 9.4
Ffryl Alcohol Eth/1 Acetate Butyl Alcohol Butyl Acetate
/'
- '" ' .
. :?.5 4.5
12.4 22.4
35
75 '
. . .. ^ _
_
- .,
. ^m
-
-
4 5 15 25
Aro;.i.itlc' Petroleum Naphtha Type 1, Grade B
gg-?....
....--g?' '
................... :. ----- i ....
. Um1'.,... , - '............,
*
-i ..
... n., MONS 092669
-
' .... ~ ...... -27, ..... . "''"''4
... ;u . .v
!?.**., .: to,:-.afflSsafiM.jWhajwtmtjmimnMWSgBr.ig
W
"v . \-.SuL." -.J&.Xs.
.v.Uwi_-*WK
10-1-44
( MONSANTO CHEMICAL COMPANY
It Is also of value In other resins uhere a highly alkali re
sistant plasticiser Is required. Papers by Bovran, Paint
Technology (reference for December 1936, dated January 1937)
Indicate many possible applications for the Aroclors. Sales
to lacquer trade at present are oonflned to specialty manufac
turers.
The compatibility of Aroclor 4465 In 1/4 second nitrocellulose
is Indicated as:
,
1. Between 24.2# and 26.5# by Inspections for blush In
thin aged films.
'
2. Between 13.7# and 16.6# by inspection for loss of
gloss In thin aged films.
,
The presence of a mutual solvent such as dibutyl phthalate raises the compatibility.
The formulation of a Tlexlble lacquer designed for oven drying Is given as follows:
(15-20 Sec. R.3. Nitrocellulose 32#
Non-Volatile 25# (Tricresyl Phosphate
4o#
('
(Aroclor 1242
28#
Volatile 75#
(Benzol (Alcohol
(Ethyl Acetate
62# 22#
16#
This formula 1b intended for application followed by oven drying.
Air drying at atmospheric temperature causes blushing. A modi
fication of the volatile portion Is suggested when air drying Is
used.
'
Volatile
Alcohol'
Ethyl Acetate Butanol Butyl Acetate
Toluol
' 6.4#
6.4# 6.4#
30.8#
50.0#
Experiments on flock Insulation and lacquers for aircraft Indi
cated Tricresyl Phosphate as a choice over Aroclors in Ethyl Cellulose lacquers, especially since there Is no tendency to
settle out when Tricresyl Phosphate Is used. Aroclor Is more effective In flame retarding, however.
Stop-Off Lacquers
Rather detailed Information is given In the Monsanto (Organic Products Division) Plasticizers and Resins Booklet on the prep aration of Nitrocellulose lacquere containing Aroclors. A -
vaftii-V?
"'IT'.
mqnS 092b70
MONSANTO CHEMICAL COMPANY
( suggested formulation Is as follows: .
10-1-44
1/2 second Nitrocellulose, Dry
Aroclor 1260
,
Trlcresyl Phosphate
Santlolser B-lo may be substituted for
Trlcresyl Phosphate
100
80-70 39-70
If the Nitrocellulose Itself does not have sufficient resistance, a composition of Aroclor with a chlorinated rubber. Ethyl Cellu lose or a Vinyl Resin again using Aroclor Is suggested, and If
the flexibility Is not sufficient, It can be Improved by the ad dition of a small amount of one of the liquid Aroolors such as
1242 or 1254, although again Trioresyl Phosphate or Santlclser B-16' could be used.
In coatings, as a general rule, the hard resinous Aroclors will produce very hard and very resistant compositions, but these will be brittle. The liquid Aroclors will tend to produce flexibility but may be lacking somewhat In adhesion. It Is for that reason that we have suggested Aroclor 1260, which Is about half-vay between and will produce a combination of flexibility and adhe sion. It will be' obvious that hardness can then be Increased by
the addition of a harder Aroclor such as 5460 or the flexibility, can be Increased by thS use of a liquid Aroclor. The Aroclors
themselves are unaffected by acid and alkali.
Stop-Off Waxes
-
The characteristics of a stop-off wax should be as follows:
a. Tightly adherent to metal surfaces. b. Should not be removed at a bath temperature of 160P.
c. Should not be'affected by the acids or alkalies of electrolytic baths. .
d. Should prevent eleatrolytlc activity on the surface covered.
e. Should be capable of removal by solvent vapor phase
. cleansing baths, by melting in boiling voter, or ordinary cleaning solutions. .
Suggested compositions are as follows:
Methlde (Monsanto Merrlmac)
Aroclor 5442
40* 60*
Softening Point
118C.
Methlde (Monsanto'Merrlmac)
Aroclor 4465
.
20* 80* -
108C.
An attempt was made to use these compositions In solution form by dissolving them In turpentine. This was not particularly
^
-89- .
'Aif HONS 092671 '-is*
HOBSAHTO CHEMICAL COMPANY
10-1 -M
successful since at room temperature the degree of solubility was lees than 12$. It might be possible to use a 25$ concen
tration of wax In turpentine at 50-75C pointing the metal J surface with the hot solution.
yAiirrg
Paints containing Aroclor have shovn remarkable durability*for better than any other .paints against vhloh they vere tested.
One serious drawback, however, Is that paints containing Aroclor do not brush as readily as the normal house paints. Paint manu
facturers Interested In quick drying paints should be encouraged to try Aroclor. Under war conditions there le great interest in the manufacture of fire-proof painting for the Interior of ships
Aroclors should be a definite contribution to their formulation.
Aroclor 5^60 is euooeesfully used In camouflage paint where It Imparts flameproofness.
VARNISHES
There has been only a limited amount of work done In our labora
tory on the subjeot of Aroclor In varnishes and from that work it
has been concluded that the moet likely field for Aroclor In
varnishes Is In conjunction with some other resin such as Ester
Oum or Dammar, or one of the other commonly used gums, since the
use of Arqolor alone has. In our experience at least, given a
tackiness to the film.
-
Aroclor 1262 mixed vlth Bast India Oum and cut with naphtha fur
nishes a varnish base.
'
The Aroclors may be used In alkali-proof varnishes by Incorpor ating them as a cold out or as a chill hack --and for the pur pose we recommend Aroclor 1262, The Aroclor may be said to function either as a resin or as an oil. In other words, by the
addition of the Aroclor, a short oil varnish takes on many of the physical characteristics of a long oil varnish. Our work
along this, line has Indloated that the best procedure Is to cook (In the usual manner) using as a resin base a pure phenolic resin hut using only half the usual amount of china-wood oil. When the
varnish attains proper body, the Aroolor may be added directly as ohlll back and the varnish then thinned iq the usual manner.
Since Aroclor 1262 le s' semi-solid resin, It Is best heated until liquid before Introducing as the chill back.
An optional method is. to dissolve It In the thinner and add In
the usual thinning operation. This was worked out a* a possible
means of extending the suppllesof china-wood oil. In other words. It acts as an.oil .substitute more than ap. a resin sub-.. .. stltute
HONS 092672
t-*us4ia
MONSANTO CHEMICAL COMPANY
10-1-44
In regard to the alkali resistance, ve have found that provided
the other materials have, of themselves, considerable alkali
resistance, then the Aroclor will add to that resistance. It Is
not possible, however, to use a resin such as limed rosin or ester
gum having poor alkali resistance and Impart high alkali resis
tance by the addition of the Aroclor.
.
Aroclor 1262 can be used to replace up to 50 of the china-wood
oil in varnishes.
-
1. If ester gum, rosin... or other cheap resin Is used, the varnish will be suitable only for Interior work.
2. If a good 1000 phenolic resin Is used, the varnish will be satisfactory for exterior purposes.
Varnishes containing Aroolor 1262 are not superior in quality to
similar varnishes made with tung oil alone, with the possible ex ception of a very slight improvement In alkali resistance, flexi bility and adhesion In some formulations.
Varnishes containing Aroclor 1262 soften at lower temperatures 'than do varnishes employing only tung oil, and'so are more sub
ject to "printing" and marring when warm.
The advantage of Increased flexibility of Aroclor varnishes Is lost, at low temperatures due to embrittlement of the Aroclor.
Because Aroclors weigh more per gallon than china-vood oil, they
Increase the cost of varnishes (which are sold by the gallon)
even if put at the same price per pound as the oil.
.
LUBRICANTS
An outstanding service Is performed by Aroolor 1254 as a lubrloant
for high pressure air compressors operating at 4400 pounds per
square Inch pressure. Besides avoiding flammability. It Is
claimed that the lubricant is superior to oil, no corrosion de
posits result, and there Is no exoesslve vear on the equipment
(Company 15850).
.
Company (233960) Is using Aroclor In a special drawing compound. Company (541370) tested Aroclor 1248 lri one of their pumps operat ing at 2500 pounds pressure with the following results: .
Compressibility change Is 0.50 compared to 0.50 for petroleum oil.
The vear rate of the pump was measured by observing the slip of
the pump at intervals during the enduranoe run. Inspection of the
pump shoved the wear, to have occurred on the. piston hole walls In
the cylinder and on the hardened surfaoe of the pintle, the sur
face of the pintle felt wavy - not smooth.' A wear rate'of 220 per
1000 hours was found to exist. The viscosity'slope of Aroclor 1248
was poor. . . ' . ' .. .
.....
: -
-
''
M0NS 092673
, MONSANTO CHEMICAL COMPANY
10-1-4*
The conclusion of these tests is reported ss follows: Aroclor 1248 is not a very satisfactory fluid for general use in oil gear pumps at 2500 pounds per square inch. It is expensive as the
pump requires special paint on the Outside and inside; the oper ating range is narrow and the wear rate on the pump tests was 22$
per 1000 hours at 100F and 25 pounds pressure.
Our experimental work in using Aroelor as a lubricant in steam ' turbines was not successful, due principally to the fact that the Aroolor is of such high density that it picks up any bit of grit that may be in the system and floats It up in ^he bearing.
Petroleum oil having so much lover density allovs most of these particles to settle in the bottom of the reservoir.
United States Patent #2,2*5,649, assigned to Celluloid Corporation, describes a steam turbine lubricant consisting of 50 parts of
chlorinated diphenyl and 50 parts,of triaryl phosphate.
- E. P. Lubricants
Much attention is being given by lubricating men to the matter of
increasing the film strength or load carrying capacity of lubri cants, particularly so as to be able to use smaller gears for a
given load
There are a great many such lubricating compounds now on the market. As a class they are called "Extreme Pressure" or E. P. Lubricants.
It is well accepted in the lubricating Industry that by the addi
tions of certain elements as Chlorine, Sulphur and others in the
proper form to a lubricating oil, a certain chemical combination
takes place with the iron or steel metal bearing surfaces. These
surface compositions tend to prevent seisure of the rubbing sur
faces under extreme loads and under vhloh loads, if the sole
lubricant was a pure mineral oil, seisure or scoring would result
at once through film failure.
,
In attempting to discuss Aroclor as an extreme pressure base, it is very difficult to evaluate its comparative load-oarrylng ,
capacities with.other extreme pressure bases, such as lead soap,
active sulphur, saponifiable oils, sulphur chloride, etc., without sotual results from exhaustive tests not only of the various
E- P. testing machines, but also from actual service under normal operating conditions. It is recognized by the lubricating indus try that results obtained on testing machines, such as Almen
machine, Timken machine and others, mean very little unless the results are correlated and proved by service conditions. It Is
true that in the past Aroclor has been tested'as an X, P. base on the Timken machine at Timken Holler Bearing and on the Oeneral
V. s-Vf * fc-iSSwJS . ...
092t>74
`.x--.. *.
jfSB
MONSANTO CHEMICAL COMPANY
10-1-AA
Motors machine at (Jeneral Motors Research, and In each case the
Aroclor addition has ahovn a marked Increase In load carrying
capacity.
'
Several companies are purchasing Aroclor today for use in 8. P. Lubricants, but indications are that they semetime add other elements along with the Aroolor to achieve commercial results at
a lower price. Since we have never run service tests on the Aro olor ourselves and the few companies purchasing Aroolor are
naturally very reluotsnt to divulge their experience along with what other chemicals, if any, they are using In conjunction with the Aroclor, the best that can be done Is to offer comments by
several of the companies who have tested the Aroclor and possibly give a general Interpretation or suggestions as to where It might find more general present day application.
Top Cylinder Lubricant
'
Recently the practice of putting a lubricant In motor gasoline
has became quite general. This Is, of oourse, to lubricate the
top section of the cylinder.
.
We have two customers who purchase Aroclor regularly for use In the top oyllnder lubricant, which they make and sell.
We do not know the function of the Aroclor In this use other then that,these customers tell us that it prevents the deposit of
carbon on the valves. Ve understand that they use a relatively small percentage of Aroclor in the lubricant.
One of these customers uses Aroclor 1248 and the other uses
Aroclor 1154.
We have- done very little work with the Aroclor as a top cylinder
lubricant but would suggest that Aroclor 1248 be used In small
percentages. This Aroolor will be found completely soluble In
low viscosity oil and should not cause any appreciable difference
In its cold test. This Is often added to the gasoline to achieve
top-cylinder lubrioatlon. .
'
Company (735900) obtained excellent results using Aroclor 1254
on a bearing test, operating in straight Aroclor at 255-260P (124-129C) for tvo weeks. Muoh less carbonisation and decom position than with the usual spindle oil under the same conditions.
. : PLA3TIC3 .
Compatibility of Aroolors with Cellulose Acetate
.
Experimental Work. The compatibility limits of Aroclor 1262 were determined with five grades of cellulose acetate, Tor these .
HONS 092675
MOIBANTO CHEMICAL COMPANY
10-1-44
cellulose acetates the limits sere as follows:
Eastman Cellulose Acetate Number
Compatibility Limit of Aroolor 1262 (per cent)
7025 7026
_ 7027 7028
10246
Between 10.0 And 13.6
Between 16.2 and 17.9 Between 13.1 and l6.b Between 17.8 and 19.7 Between 16.4' and j8.1
These figures, as well as all the compatibility limits given In
this report, refer to the limits as determined on thin films dried slowly In dry air and deposited from solutions containing, as Is customary, 0.1 gram of "solids" per cubic centimeter of
solution. The solvent was a mixture of 80$ by weight of ethylene dlchloride and 20jC of alcohol (denatured. Formula 3A).
Another solvent mixture comprising 33.3# acetone, 33.3J6 ethyl lactate, 16.756 alcohol and 16.7)6 ethyl acetate (all percentages
by weight) was less suitable than the solvent given above, and gave lower compatibility limits in the cases tried.
Tne compatibility limits of several Aroclors with one cellulose
acetate (#10246) were determined. The observed limits were as
follows:
- -'
Aroclor No.
Limit (Per cent)
1242 1254 1262
4465 5465
.
From 25.9 to 28.7 From 25.7 to 29.1 From 16.4 to l8.1
From 14.2 to l6.8
From 10,1 to 13.0
The ternary systems, comprising a cellulose acetate, Aroclor 1254,
and a common plasticizer, were Investigated.
'
The constants of the oellulose acetates, 'as given by Eastman
Kodak Company, are as follows:
-.-.y ' ....... ....... .
.Cellulose
Aeetyl
Acetate Ho. (Per cent
Viscosity (Seconds]
'<
MONSANTO CHEMICAL COMPANY
10-1-44
Conclualona
The compatibility limits of various Aroolors In a specific cellu lose acetate and or one Aroclor in various oellulose acetates are
comparatively lov. The type of solvent employed affects the ob served limits, *he solvent whloh gives the more favorable results being the mixture of ethylene dlohloride and aloohol. The com patibility limits of the Aroclors in oellulose acetate are. In general, more dlffloult to determine and less readily checked
than the limits In nitrocellulose. The actual- observed limit apparently depends upon the rate of drying, the thickness of the
deposited film, the humidity of the air, and the solvent employed.
In the tests of compatibility made by Eastman Kodak Company, the limits were found to be 50 to 100 (Rittenhouse). Their lov re sults vere probably due to their method of detecting Incompati bility, In which delicate optical methods vore employed to detect
hate In the film.
The work on the effeot of Aroolors upon the rate of burning of cellulose acetate films, as given In the table, leads to the following conclusions:
1. Cellulose Acetate alone' burns slowly.
2. The rate of burning, where burning takes place at all-, is accelerated by each of the substances tried.
3. While the Aroclors Increase the rate of burning, they at the same time give a flickering uncertain flame' vhlch
. tends to go out, that Is, they tend to quench the flame,
4. Trlphenyl Phosphate Is an effective flameproofer. It be ing Impossible to Ignite the film containing 250 of It.
5. If flexibility and lack of tendency of the film to wrinkle or curl on drying is taken as a criterion of plasticising power, -the Aroclors are more effective plasticisers than ' either dibutyl phtbalate or Trlcrosyl Phosphate.
6. The thick film containing 250 Aroclor 1254 (slightly
below the compatibility limit for thin films) was blushed. This is In acoord with the earlier observations of the effect of film thickness on the compatibility limit.
Company (756593) has found that mixtures of decachlorodlphenyl '
and styrene are non-lnflassnable and have a heat distortion point
20P higher than polystyrene,
'.
.
United States Patent No. 2,227,637, assigned to Leverkusen-I.O, . Verk, describes a composition of matter comprising a realn-llke
chlorinated diphenyl of an average chlorine content of about 620
HONS 092677
MONSANTO CHEMICAL COMPANY
10-1-44
and about 7.50 of polyvinyl earbasole.
RUBBER
Company (.297400) have found that Aroclor 1262 la the beat plas
ticiser for rubber hydrochloride. It la compatible up to 1000
rubber hydrochloride, although the ueual working range la 5 to
100 of Aroclor 1262 baaed on the weight of the ohlorlnated rubber.
Below 500 Aroclor no difficulty la encountered with brlttleneaa.
Aroclor tenda to lncreaae the gloss of rubber hydrochloride fllma,
e.g., Pllofonn, Pliofilm, Pliollte. Five por oent rubber hydro
chloride added to Aroclor reducea the tack.
.
-
On tho other hand. Company (331850) recommends the uae of Aroclor
1254 with chlorinated rubber, e.g., Parlon.
yt--v~r
A rubber oompoaltlon of reduced flammability comprises
>**.
Rubber
.
Chlorinated rubber
Aroclora
Sulfur
Zinc Oxide
'
Vuloanlclng Accelerator
Ammonium Borate
100 parte
35 parte 65 parts
2.8 parta
5 porta 1 part 40 parte
Th]? composition above a flame resistance'and a notable absence of melting around the burning material.
Aroclor 1268 la used In the manufacture of Cellular rubber of low flammability for the aircraft Industry.
Company (284144) has found that 150 of Aroclor 1242 added to
Vlstlnex (polybutene) makes a de-lclng coating for airplane pro
pellers that looks promising. By the addition of plasticiser
C-2V or plasticiser SC, low temperature characteristics can be
obtained.
. .. ..
It is Indicated that Aroclor 1242 may act as a solvent for one of the materials which la producing tack in Buna 3.
The characteristics of Type B Keoprenp compositions are said to
be improved by the addition of Aroclor 1254 Increasing water
resistance. (Company 16947) , ..
,
The use of Aroclor 5160 Is under Investigation as on extender for
Hycar OR.
' :
There are several different applications for Aroclor in rubber
as follows:
-
- .
- ; -vs.,
..
`
r MONSANTO CHEMICAL COMPANY As a plasticizer for hard rubber
10-1 -44
Aroclor 1262 has been used as a plasticiser for bard rubber In dental plates, eto., for a couple of years. It should be equally useful In plasticising herd rubber for other purposes vhere brittleness Is undesirable.
To render rubber permanently tacky .
.
Aroclors 1262 and 1254 are milled Into rubber' so as to make a homogeneous compound vhlch has permanent tackiness or adhesion.
To flameproof rubber. Neoprene, and other synthetic rubbers
Aroclor 1269 Is a hard crystalline material of high melting point.
It may be ground very fine. This finely ground Aroclor Is milled
Into the rubber Just as any Inert filler vould be. The milling
temperature Is not high enough to melt this Aroclor and so there
la no solvent action. It has been found that the Incorporation
of sufficient Aroclor 1269 in rubber prevents the spread of flame.
This Is suggested especially for flameproofing rubber for use on
Insulated vlre.
.-
. THERMOSTATS
C Aroclor 1248 Is being used by several manufacturers of thermo stats as the expanding medium In the bulb. Aroclor has been used In this service by one manufacturer for the last ten years.
Aroolorhas proved entirely satisfactory. Every precaution must be taken to eliminate the possibility of moisture or other for eign matter getting Into the Aroolor. The thermostat equipment must be thoroughly cleaned before filling.
We do not recommend the uBe of Aroclor at temperatures above
600OP (3150c).
...
TEXTILES
Company (645300) reports that Aroclors^ although more expensive,
exert better fire retardant offeot than chlorinated paraffins
and smaller amounts are required.
........
Company (049900) claimed that Aroclors 1262 and 5460 shoved a lOJt Increase in tensile strength vhen substituted for the stand
ard Jeffersonville Quartermaster Depot specified impregnant for rope, vhloh Is the follovlng formula:
4ljl Copper Naphthenate 800-8 98J6
14 Asphalt
- ' - -......
30)t Paraffin Wax
.j
15* Mineral Seal Oil
-
10-1-44 MON3AUTO CHEMICAL COMPAJW (
Aroclor 1260 Is proposed as a flameproofing, waterproofing, mlldewprooflng agent In the production of J.Q.D.'s specification 242 paullns and tentage for army use. Exact formulation'and approval of the Quartermaster Corps has not yet been worked out.
' WOOD
Aroclor as an Introfler for Sulfur In Wood Impregnation
It has been found desirable for some purposes to Impregnate wood
and other fibrous materials with sulfur. However, sulfur does
not go Into these materials without difficulty. The use of 10$ .
of Aroclor 4465 mixed with the sulfur aots as an Introfler, caus
ing thorough penetration.
.
.
The Impregnation is performed as followst
A mixture of 90$ sulfur and 10$ Aroolor 4465 la melted and mixed I Aand placed in an autoclave or pressure tank with the wood or other material to be Impregnated and held at a temperature of 125C to 140C and a pressure of 100 pounds per square Inch. The time necessary depends upon the kind of wood or other material being treated. The Initial fredslng point of this mixture Is 107.5C. , The viscosity at 125C Is reported as 27 Seconds Saybolt Universal. /
(' A typioal impregnation of a yellow- pine 2" x 8" plank gave an Increase In weight of 127$ and about 100$ in tensile strength.
The valuable qualities contributed by this treatment are added strength, rigidity, resistance to moisture, to acids and to
splintering. The electrical Insulating properties are Increased. The wood Is made practically free from the effect of weather and
resists attack by lnseots. The treated wood Is practically free from shrinkage and swelling.
Possible uses of wood treated in this way are:
Transmission line crosaarms.'
Tanks to resist aolds, etc.
Equipment In which swelling or splintering Is objectionable.
Timbers likely to be attacked by termites, etc.
Perhaps many other applications where the qualities
described above are desirable:
-
The requirement Is that the wood so treated Should stand being :
l. used 15 or 20 times In concrete forms, that, it must remain smooth,
and not show annular ring or grain structure' 00 the concrete
.
1
MONSANTO CHEMICAL COMPANY
10-1-**
where the forms are used. Plywood Impregnated with a mixture
of Aroclor 2565 and 10-20$ hard paraffin (melting point 60-68C)
would be suitable for the construction of concrete forms. Addi
tion of suirur up to 200 of the mixture may be beneflolal In
reducing the cost of Impregnating material and In making the
treated wood harder.
,
The reoommended procedure'consists of keeping the plyvobd sub merged for 30 minutes In the Aroclor-Paraffln mixture (or Aro clor, Paraffin, Sulfur mixture) at 80-90OC, then letting the
boards drain at about 50C and passing them between rollers to wipe off the excess of the wax.
Plywood treated In this sianner Increases In weight from 37 to 66$
and gains only 3.1 to 5.7$ In weight when Immersed in water for
six hours. Untreated vood gains 29$ in weight when kept In water
for an equal length of time.
'
Standard maple vood blocks used by the shoe last Industry from (Company 769520) were treated with various compounds to prevent
dimensional change from water absorption. The most effective composition was found to consist of:
70$ Aroclor 2565 20$ Paraffin (hard or soft)
10$ Sulfur '
.
When this composition was applied under the conditions shown be
low the results Indicated were obtained:
-
Effect of Soaking
In Water 24 hrs.
Weight of
" - [ $ Per-
Treatment . Oain'lnWt. Imeter
mg/sq.in.Surface g/sq.Heter Change
1.- 60 min. at 100C. 1;
30 min. cooling
-
2. 60 min. at 100C.; . 30 min. cooling
3. 60 min. at 100C.j ' 30 min. cooling -
4. 60 min. at 100C..j . .
30 min. cooling
1' -
5. Vac. 30 min. at 90C 5 min.. released 10 min .
Maximum tolerable limit
*5.36
3*0 ,
0.3*9
*2.96
375 0.3*9
*9-26
. 351
0.3*9
*9.50
367,
0.525
36.*9 - v;:- *87 . , / 0.175 ......, _v v : 0.556
MONSANTO CHEMICAL COMPANY
10-1-4*
From another series of tests conducted on hickory fishing pole
handles It Is concluded that the best results will be obtained
using the following conditions!
Temperature Vacuum Atmospheric pressure
Remove, drain and dry
90-100C 16-100 am. for 25 min. 5 min.
''
.
-.
MISCELLANEOUS ...
"
Purdue University found that Aroclor 1242 was very useful as a
base upon which to flow gelatin solutions for the production of
films, thus making It possible to eliminate mercury for this
purpose.
As a result of Interest aroused In the Aroolors, several sugges tions have been made regarding uses which may prove of value.
1. Aroclor 1260 as an adhesive In a Joint compound for glass
building blocks.
,
2. A water emulsion of Aroolor 1262 for use In leather, paper, . textiles, rubber and casein paints.
3. As a protective coating on certain pigments to prevent "llverlng" of paints containing resins of a high acid number. Specifically, sine oxide pigment In water emul
sion of "Aquaplex," a water emulslflable alkyd resin.
4. A waterproofing for concrete.
5. Aroolor 1262 or 5460 as an Ingredient of molding' eomposl-
tlons made with such materials as ethyl cellulose, bensyl
cellulose, soy bean meal and corn protein.
'
. '
(
MONSANTO CHEMICAL COMPANY
10-1-44
SUGGESTED FORMULAE FOR MOISTUREPROOFING '___________ COMPOUNDS________ _____
Compound A Compound B Compound 0 Compound D
96.056 Aroclor 5460 4.0)6 Bard Paraffin
96.0ft Aroclor 4465 4.0jf Hard Paraffin
96.0)6 Aroclor 5060 4.0)6 Hard Paraffin
96.0)6 Aroolor 4o65 4.0j6 Hard Paraffin
When a relatively low softening point material la de sired, we suggest those compounds using Aroclor 4465.
When a higher softening point Is required, we suggest the compounds using Aroclor 5460.
Compounds C and D are black materials and are useful where oolor Is of no Importance.
Ve do not prepare these compounds.
'
HONS 092683