Document 5bnVjJKrDj0z2GjKYZMzDpppV
Q.
;> -U
-
;C
MASTER COPy
A i * . *
OF AROCLORS AND THEIR MIXTURES IN THE ? ELECTRICAL INDUSTRY
, , ;v- . -A:..
-^v.U-Ti*. * . .
t;. ; ^ t :
?M!>
Mo^ntt Monoi)+oChmkoT:Cei, Organic Piv, Sain font.
LA/L-J 800. N, lln^rjh tUi. St, 18, lli.f
P, C. 0EN10NU*
R !<
..
Jinvary 19&0 ,
i*
'-i*f 4-*,. -tV
0263127
TOWOLDMON0028581 WATER PCB-00013050
INDEX
Introduction - Page 1-2
Chapter 1 - Page 3-12
Page 3 Page 4 Page 12
Chapter 2 - Page 13-19 Page 13 Page 17
Chapter 3 - Page 20-21A Page 20
Page 21
Chapter 4 - Page 22-25 Page 22 Page 23 Page 25
Chapter 5 - Page 26-28 Page 26
Chapter 6 - Page 29-61 Page 29 Page 31
Page 31 Page 32 Page 38
The Proper Handling Of Aroclors And Their Mixtures In The Electrical Industry
Procedure For Unloading Tankcars Of Aroclors And Aroolor Mixtures
(A) Description of the Cars (B) Procedure for Unloading the Cars (C) Drum Packaging
Storage Tanks
(A) General Description (B) Detailed Description
Gasketing and Pump Faoklng
(A) Suggested Types Of Packing and Qasketlng Materials
(B) Gaskets For Askarel Capacitors and Transformers
Sampling Methods
(A) The ASTM Standard Method iB) Monsanto Methods (C) Drum Sampling
Laboratory Analysis and Procedure
(A) For Treating Aroclors and Their Mixtures with Earth
Test Procedures
(A) General Information (B) Detailed Instruction and
Testing Methods
1. Procedure for Cleaning Electrodes
2. Dleleotrlo Constant and Power Faotor
3. Dleleotrlo Strength
02631.28
TOWOLDMON0028582 WATER_PCB-00013051
Page 44 Page 47 Page 49 Page 51 Page 52 Page 55 Page 59
Chapter 7 - Page 62-73 Page 64 Page 65 Page 66 Page 67 Page 68 Page 69 Page 70 Page 71 Page 72 Page 73
Chapter 8 - Page 74-76
Page 74
Page 74 Page 75
Chapter 9 - Page 77-79
Page 77 Page 77 Page 78
Page 79
4. Resistivity
5. Corrosion and Chemical Stability
6. Xnorganlo Chlorides
7. Acid Number 8. Moisture 9. Hydrolysis Stability Test
for Aroclor 10. Thermal Stability Method
for Aroclors
Typical Properties
Aroclor 1232 Aroclor 1242 Aroclor 1248 Aroclor 1254 Aroolor 1260 Pyranol l48l Pyranol 1488 Pyranol 1467 Pyranol 1470 Inerteen PPO
Quality Requirements of Aroclors Prior to Use In the Electrical Industry
Quality as Supplied to the Hlectrioal Industry Typical Electrloal Quality of Aroolors Used In the Industry Capaoltor Impregnation Transformer Filling
Earth Refinement of Aroclors to Arrive at the Desired Elec.trlcal Qualities
Earth Treatment in the Laboratory Preparatory to Analysis Earth Treatment by the Plant Manufacturing the Askarel Earth Refinement by the User
Capacitor Manufacturers Transformer Manufacturers The Effect of Earth Refinement on Removal of Tin Tetraphenyl Scavengers from Transformer Askarel
0*63129
|
TOWOLDMON0028583 WATER_PCB-00013052
Chapter 10 - Page 80-93 Page 80 Page 83
Contamination
Avoidance of Contaminating Askarel Capacitors Avoidanoe of Contaminating Askarel Transformers
Chapter 11 - Page 94-97
Page 94 Page 95
Reworking Contaminated Transformer
Askarel Normal Conditions Arced Conditions
Chapter 12 - Page 98-100
Page 98 Page 99 Page 100
Dermatology and Toxloology
Skin Exposure Exposure to Vapors Vapors from a Severely Arced Askarel Transformer
Attachments!
Drawing No. 31-20847/ The Tank Car Drawing No. 31-20848; Dome Detail Drawing No. 0-8170-5; The Horizontal Storage Tank Drawing No. D-13362, The Vertioal Storage Tank Drawing No. 90-8248; The Breather
Drawing No. 9C-8278; The Vareo Gauge Drawing No. 9C-8178, The Unloading Platform
0263130
TOWOLDMON0028584 WATER_PCB-00013053
THE PROPER HANDLING OP AROCLORS* AND THEIR MIXTURES IN THE ELECTRICAL INDUSTRY
INTRODUCTION
Monsanto's Aroclors*, especially the chlorinated biphenyls
1016, and
including typesA1242y
1254,attd-1-060^ used alone or in
combination with chlorinated benzenes, are commonly used die lectric materials of the askarel^ class.
Askarel is a generic name referring to liquid dielectrics derived from halogenated aromatic hydrooarbons possessing excellent chemical and dielectric stability and fire-resistance over the temperature ranges and operating conditions required of transformers and capacitors in the electrical Industry.
The properties of Aroclors and their mixtures, used as dielectrics are described in detail in Chapter 7 entitled, "Typical Properties". These dielectrics are manufactured under very carefully controlled conditions in order to meet the strict and exacting electrical requirements and properties.
The electrical industry's use of these fluids has been largely in accordance with the General Electric Company's patents and developments.
"Aroclors - Monsanto's chlorinated biphenyls and chlorinated polyphenyls, Registered U.S. Patent Office.
1F. M. Clark, "Electrical Insulation". Chem. Engg. News 25. 2977
(1947).
-----------------
-1-
0Z63131
|
TOWOLDMON0028585 WATER_PCB-00013054
Resulting from the wide use of these materials In the Industry, trade names have been established to Identify them by different manufacturers of electrical equipment. Listed alphabetically the trade names Include, "Chlorextol," Allis Chalmers; "Dlaclor," Sangamo Electric; "Dykanol," Cornell Dubilier; "Elemex," Line Materials; "Hyvol," Aerovox; "Inerteen," Westinghouse Electric; "Noflamol," Wagner Eleotrlc; and Pyranoi," General Electric Company.
The purpose of this bulletin is to assist the industry with the proper and safe handling of these dlelectrio materials In their operations.
0263132
TOWOLDMON0028586 WATER_PCB-00013055
CHAPTER 1
PROCEDURE FOR UNLOADING TANKCARS OF AROCLORS AND AROCLOR MIXTURES
A. Description of the Cars Aroolor and mixtures of Aroolors with chlorinated benzenes
are shipped by Monsanto In two types of insulated tankcarsboth of which are either aluminum lined or zinc-tin metallized. One type of car has heating colls Inside of the tank and these are in direct contact with the product. The other, a more widely used type of car. Is a double-shell tank with heating colls between the Inner and outer shells. The steam coil connections are at the bottom of the car. Both types of tankcars are tested for 60 pounds pressure and their steam coils are tested for 200 pounds gauge pressure.
The cars are top-unloaded by displacement with dry air containing 10 mg. H-O/cu. ft. maximum.
There are two or three connections on the tankcar dome depending on the type of car. Where three connections exist, one Is a two inch diameter unloading line whioh extends to the bottom of the car, the second is a one inch diameter air inlet connection and the third is a two inch diameter pressure safety vent, which is a thin lead disc adjusted to release any pressure in excess of 60 pounds gauge. This safety vent is hooded for protection against dust, dirt or accidental bumping.
Where only two connections exist on the dome, one is the two inch diameter unloading line and the other 1b the safety vent. On these cars, it is necessary to remove the safety vent and introduce the displacement air through that connection.
-3- I TOWOLDMON0028587 WATER_PCB-00013056
0263133
***#
While the tankcar drawing gives, much detail, we have been asked about the following points not given in the drawing:
1. The distance from the rail track to the top of the dome of the cars is variable. It is 13 feet and 4 inches for the 7^000 gallon cars and ranges from 11 feet to 14 feet for the 8,000 gallon cars.
2. The steam connections are located under the center of the cars.
3- The steam pipe connection is usually a two inch pipe, but on some cars the pipe Bize is 1-1/4 Inches.
4. American Standard taper pipe threads are used.
*# *
-3A-
0263134
I
TOWOLDMON0028588 WATER_PCB-00013057
Drawing No. 31-20^48 shows in detail the dome of a tankcar with three connections. "A" 1b the two inch unloading line which extends to a email sump at the bottom of the car. "B" is the one inch air inlet connection. "C" is the hooded safety vent. The car dome cover with fitted boltB is shown in the center. It 1b fitted with an aluminum envelope Goetze gasket v A series soe Oarlock. asbestos gasket. This drawing also shows a bottom opening in the oar. ThiB can be opened only from the Inside of the car and its purpose is for oleaning operations, it has no ubs at all in unloading the car.
Drawing No. 31-20847 shows the overall dimensions of the 8,000 gallon Aroclor tankcar.
B. Procedure for Unloading the Cars The car should be spotted at an unloading doek similar to
the one shown by Drawing No. 9C-817B. The oar must be level and the brakes set properly. "STOP - TANKCAR CONNECTED" signs should be placed fore and aft the car to warn switching crews.
If it is raning or snowing or the humidity is extremely high. It is not advisable to open the car. In case the car must be sampled and opened during bad weather, a canvas canopy must be placed over the dome of the oar. It is preferable to unload the cars under roof or inside the factory. Unless it Is absolutely necessary because of following described situations the dome cover should not be opened until ready for sampling. The dome cover is sealed with a standard railroad wire and seal, and Monsanto should be notified if this seal is found broken upon receipt of the car.
OZb313,5
I
TOWOLDMON0028589 WATER_PCB-00013058
The first step in unloading ia to inspect the dome and
clean around the dome cover to remove all looBe dirt, water or
snow. Wiping rags and a brush should be used to clean before
the dome cover and connections are opened.
Then, the screwed hood over the alr-lnlet valve should be
removed and this valve opened fully and left open while hebtlng
the car. A Weston or metal encased thermometer should be
inserted through this air-inlet valve opening and the tempera
ture of the interior of the car determined.
If the car temperature is below the caution temperature
shown in the following Table 1, it will be necessary to take
the special step of inserting a "hair-pin" heating coil through
the dome of the car to preclude rupturing the tankcar seams
during the heating period.
TABLE I
Product
ASTM Pour Point C.
Temperature C. Below which Caution Must Be Deed in Heating
Arooler 1060~
+ 40-*-
Aroclor
+ 20
Aroalor-
i vAroclor 12^2
.-s- 19
- / 0 ---- 10
pro clef lot ( 7^nerteen we^io/jo "^re-heating is not required;*,
-^Pyranol ljl6?~r-
~ > fpre heating is not required
v-#
Pyranol Pyranol
l470~r13 635-3
Pre-heating is net required Pre-heating is not required*
- <0
Except if the material has cooled below -10C. and crystals of scavenger have separated. Then,
the material should be heated to 70C. (158?.) until complete solution has been accomplished.
0263136
I
TOWOLDMON0028590 WATER_PCB-00013059
If the dome of the car is to be opened for the pre-heating operation, it is necessary that it be covered with a clean canvas. Extreme care must be taken to avoid getting dirt or moisture into the car.
It is due to the relatively high viscosity of some of the Aroclors at low temperatures that it becomes necessary to form a column of molten material from top to bottom of the car, in the center, to prevent hydraulic pressure build-up which may rupture the tank shell if there is too rapid localized heating when employing the main steam coils.
When such pre-heating is required, a satisfactory vent hole can be made by inserting a "hair-pin" coil (1/2 inch diameter brass, galvanized, or stainless steel pipe) into the open dome of the car and Introducing steam through the coil until there is a column of fluid Aroolor from top to bottom.
After the vent hole is melted through the material to the bottom of the car, the "hair-pin" coil should be removed and the dome cover replaoed and bolted.
Steam is then introduced into the main coils. It is recommended that the steam pressure be limited to 100 pounds gauge pressure, particularly when the coils are in direct contact with the Aroclor. The steam coil outlet should be trapped or throttled with a valve.
It will require eight to twenty hours to bring the material to pumping temperature - depending upon weather conditions. it is essential that the air inlet valve be open during the heat ing period in order to vent the tank.
TOWOLDMON0028591 WATER_PCB-00013060
Some calculations have been made to Indicate the heat
requirements for an Aroelor car. Data for an 8,000 gallon
car of Aroelor 1254 ares
Specific Oravlty Specific Heat
= 1.5 = 0.26 Btu/lb./F.
Heat requirement for heating Aroelor from 30C. (86P.) to
110C. (230F.) lss
8000 x 1.5 x 8.33 x 0.26 x (230-86) = 3,774,000 Btu.
For heating from 30C. (86F.) to only 75C. (1670F.), the
heat required Is 2,110,000 Btu.
A nine horse power boiler operating at 80 pslg produces
263 lbs./hr. of steam with no reused condensate. Returning
condensate at 200F. will Increase the steam output to 296 lbs./hr.
at 80 pslg.
In the first case, heating to 110C., the over-all heat
transfer co-effiolent Is assumed to be too low to utilize the
iOO# capacity of the boiler. A value of 1500 for DA with an
average h T of 133F. indicates that the useable steam Is
202,000 Btu/fa>. or 226 lbs./hr. steam at 80 pslg.
In the second case the ^ T Is lower and the entire
output of the boiler is useable. TaBe II sums up the approximate
time calculated to heat Aroolor 1254 in an 8,000 gallon car.
-7- 263138
TOWOLDMON0028592 WATER_PCB-00013061
TABLE XI
Nine HP Boiler
Lbs. Steam/Hr. 30-110C. 30-75C,
100$ cap. (no reused condensate)
263
-- 9 hrs,
75$ cap. (no reused condensate)
--
18 hrs.
12 hrs
(86$ cap)
100$ cap. (condensate 9 200P.)
296
-- 8 hrs
75$ cap. (condensate 9 200P.)
--
18 hrs.
11 hrs
(76$ oap)
Calculations on a five horse power boiler give heating times of the
following order:
Five Hf Boiler
Lbs. Steam/Hr. 30-110C. 30-75C
100$ cap. (no reused condensate)
146
28 hrs.
16 hrs
100$ cap. (condensate S 200F.)
164
25 hrs.
14 hrs
Aroclor cars can be heated by steam (80-100 psig) to the proper
handling temperatures In a reasonable time by using a boiler source
capable of producing 200,000 to 300,000 Btu/hr. The times given here
are approximate and will act as a guide until experience Bhows the
exact time for this operation.
o*bVV3
TOWOLDMON0028593 WATER_PCB-00013062
The proper handling temperature for the various fluids Is given In the following Table III, whloh IndloateB correspond ing viscosity values:
TABLE III
Product
Handling and Pumping Temperature C.
Approximate Viscosity, S.U.S.
Aroclor 1254 Aroclar 1248 ~~f-
93-----75 - HO
19----- 43100 - 42 406------4-*-
Aroclor 1242 Arottor I0l6 Pyranol 1*18-1 pyrene/ A13B30-3 Pyranol 1/16?--*-
Pyranol l470--
35 - 75 30 - ''-T
30 - 75 ao - SS
100 - 40 100 - *iO 100 - 40
406--4cr
1QQ -4^
Inerteen -PP-* 10/30 Inrtee to3*' - W
100 - 40 100 - so
*If any of the scavenger Is out of solution, then the material must be heated at 70C. (15SF ) until
It has dissolved.
Selection of pumping temperatures for any dielectric not
shown on this list or which may be developed In the future should
be based on a viscosity of about 100 Saybolt Universal Seconds
for average pumping and about 40 S.U.S. for fast pumping.
When the material has been heated to pumping temperature,
a one-half inch diameter pipe "oross" arrangement containing
a pressure gauge, air inlet, pressure relief valve to relieve
at 30 Psig, and vent connections, should be connected to the dome
air Inlet pipe. Then the unloading line should be connected. Aluminum or
Rust-free and clean galvanized piping ordstainless steel pipe
should be used for the unloading line.
opeai'to
^
TOWOLDMON0028594 WATER_PCB-00013063
(At this point a sample is taken as described in Chapter 4,)
Dry* air is then introduced into the tankcar and pressure built
up to 15 pounds gauge. The two inch valve cook on the stand pipe
is opened and the discharge pipe observed to be sure the
liquid is being unloaded. To protect the seams in the tankcar,
the pressure must not exceed 30 pounds. The car will begin to
unload at about 12 pounds pressure.
When the oar is empty, the air pressure will drop off
rapidly and air will blow out of the vent on the reoeiving tank.
The air flow may be stopped at this point and the tankcar
pressure released through the vent valve on the "cross" arrangement
After inspecting the car to be sure that it has been completely
unloaded, all connections and dome cover should be closed
tightly, it is essential that the empty tankcar be sealed
immediately after the car is unloaded in order to keep the car
filled with dry air during return Bhipment.
*It is essential that the displacement air used for unloading be dried thoroughly by some dehumidfylng unit such as soda lime, activated alumina or similar dehydrating agent drying unit. It may be necessary to recharge the dehumidlfying unit each time that a oar is unloaded. For unloading a tankoar of Aroclor within three hours, 15 standard cubic feet a minute of air at 15 pounds per square inoh gauge pressure and a -100F. dew point should be supplied. If the dry air unit is to be used only for unloading tankcars, a small single tower dryer unit containing a selfcontained reactivating heater is suggested. Two manufacturers of air dryers of this type are: C. M. Kemp Mfg. Co., 405 E. Oliver Street, Baltimore 2, Maryland and Pittsburgh Lectrodryer Corporation, Foot of 32nd Street, Pittsburgh, Pennsylvania.
-10-
ozes!*1
TOWOLDMON0028595 WATER_PCB-00013064
As a final step. It Is desired that a standard railroad
wire seal be Inserted through the Blotted bolts of the
car fittings. Steam should be released from the oar
colls and all condensate removed from the colls by
blowing with air with the steam trap by-passed. All
connections must be replaced as received. Adequate oare
should be taken In preparing and sealing the car for
return shipment.
Unloading with dry air as desarlbed Is the preferred
and recommended procedure because It Is done with the oar
dome closed whloh avoids contamination.
Dry nitrogen may be used Instead of dry air. If
nitrogen is used It is essential to notify us (the supplier)
so that we oan take required safety precautions relative
to replacing the nitrogen with air In the returned oar prior
to sending our men Into it for cleaning.
If the oar Is unloaded by pumping out of the top, whloh
required opening the dome, It Is most desirable that the car
be set Inside of a building. If this oannot be done, then
a canopy or roof should be provided over the oar dome, and
the unloading should be done when the weather Is dear.
A clean centrifugal pump with minimum capaolty of
40 gpm. Is suggested. It will be necessary to prime the
pump and only clean askarel should be used to do this.
Another method for priming the pump Is to use a Penberthy
steam Jet, Mo. 22A available from Penberthy Injector Co.,
1242 Holden Ave., Detroit 2, Michigan. (Further pump detail
is given on page 17)
- 11 -
^31V
TOWOLDMON0028596 WATER_PCB-00013065
C. Drum Packaging
Drum packaging Is made with new and carefully Inspected
55-gallon drums. These steel drums are lined with a specially
tke Stfiet 'll e.)ci9r ep*y phe.nl``-
selected baked phenolic coating. An example laANESCO Me. 3 *-
BrA^tey V^oomAA Oivision l tOhi'lt Aker-
lining offered by theANatlonal Enameling and-Stamping Company) aW^aai
CKunjo, Illinois.
Jrtlmmm
Dong--Island, Now Yorlu^ Contents of the drums should not be
heated by direct application of flame or strip heaters. Radiant
heat from steam colls or hot air In a heated room Is to be
preferred. The screw plug In the drum head is fitted with a
metal cap sb a safe guard against tampering.
The drums should be stored indoors. If outdoor storage
cannot be avoided, the drums should be placed In a horizontal
position and covered with a tarpaulin.
-12'
02fc31'*3
|
TOWOLDMON0028597 WATER_PCB-00013066
CHAPTER 2 STORAGE TANKS
A. General Description The storage tanks should be a minimum of 10,000 gallons
and preferably 12,000 to 15,000 gallons capacity to accommodate the normal 8,000 gallon tankcars.
It is preferable to locate the tanks above ground where they are easily accessible for any ohanges or repairs. Underground location presents difficulty in this respect.
Especially in cold climates, it is preferable to locate the tanks inside of a building. The tanks should be located conveniently with reference to the tankcar unloading facilities and the area where the dielectric is used.
Although Aroclors are non-corrosive to metalB, corrosion or rusting of iron and steel equipment (by oxidation) may occur resulting in contamination of the products. The resistance of Aroclors to materials of construction is given in Monsanto Technical Bulletin, OP-115, entitled, "The Aroclors", Page 6.
Stainless steel tanks are very satisfactory but relatively expensive. Stainless steel pipe is relatively difficult to fabricate and it is difficult to make tight leak-proof connec tions .
Storage tanks may be of steel construction if properly metallized with zinc-tin or aluminum on the interior surfaces coming in contact with the Aroclors.
-13-
0263144
TOWOLDMON0028598 WATER_PCB-00013067
The metallizing should be done according to the following procedure:
1. Clean an area of the surface by sand blasting,
or a similar method to give a perfectly dean and roughened surfaoe. The area cleaned should not be greater than can be completely metallized within a few hours after oleaning.
2. If zinc-tin metallizing Is used, a ooating of zinc 0.005 inches thick should be sprayed on to the cleaned Burface. This Is followed immediately by a coating of tin 0.007 inches thick.
3. Aluminum metallized surfacing should be about 0.01 inch thick.
The detailed procedure for metallizing and cleaning is out lined as follows:
a) Sand blast, b) Coat with iron, 0.005 inohes thick. (The purpose of this ooating is to provide a rougher and better bond
for the finish coat of aluminum or the zinc-tin combination.) c) Apply the selected finish coat, d) Pill the tank with tap
water and warm it with steam. (If an open steam line is used, do not allow the steam to impinge dlreotly onto the metallized surface of the tank.) e) Drain the tank, f) Pill with cold
water and drain, g) Klpe dry and clean with clean diaper cloth or other fabric relatively free of lint, h) Heat the tank to at leapt 100C. (212F.) to expell moist air. It would be benefi
cial to heat the tank, allow it to oool and pull dry air through it using a dehumidfying breather in the air line, heat again
etc., until the tank is full of comparatively dry air. 1) Spray about 100 gallons of new, eleotrloal grade Aroclor (not high in viscosity) or electrical grade triohlorobenzene onto the inner
walls of the tank, washing the walls thoroughly (avoid breathing
any fumes), j) Attach the circulating pump, the lines used, and
-14-
~"
02631*5
TOWOLDMON0028599
WATER_PCB-00013068
the filter press fitted with dry paper and oirculate the fluid
through the system and the tank. Install new dry filter paper
several timeB in the press during this drying and oleaning
operation. Discard the dielectric fluid used for cleaning,
k) Partially fill the tank with new Aroclor dielectric and
analyze it eleotrically and chemically to determine whether
it meets specifications. If all tests are met, then fill
the tank with the dielectric.
The tanks should be Insulated using, preferably, glass
foam beads as supplied by Dow-Corning or Llbby-Owens-Ford.
The suggested thickness of the glass insulation is one inch
minimum to two Inches maximum. The glass insulation may be
covered with tar material commonly used for weather-proofing.
Another type of Insulation which may be used instead of the
glass is 85# Magnesia-Wool which should be covered also with
the weather-proofing tar. Hie advantage of the glass insul
ation is that it is not moisture sensitive as is the case
with Magnesia-Wool.
If the storage tank is located outdoors, it is best that
the insulation be covered with riveted or bolted tin sheeting
painted with aluminum pa.int. This type of metal surface
weathers well and is cleaned easily. All piping must be stain!*si,
ulupi'nxm r
--
A galvanized.andicrewed fittings must be back brazed to assure
tightness. All handling pipe lines must be traced with steam
lines and insulation applied over the two lines in order to
keep the handling lines and the material up to the desired
pumping temperature. Usually a one-fourth inch copper steam
line running parallel with the handling line will suffice.
*
-15-
02631*>
TOWOLDMON0028600
WATER_PCB-00013069
Under very severe conditions of low temperatures, it would be
desirable to wind the steam line around the handling line about two turns to the foot.
The tankB must be provided with ample pressurized heating
coll surface to supply sufficient heat to the material to
bring it to the proper temperature for pumping and handling
as indicated in Table 111. Heating oolls should be either
metallized steel, or preferably steel coils which have been
galvanized after fabrication. It is recommended that the
steam pressure on all heating ooils should not exceed 100 pounds per square lnoh gauge; lower pressures may be used
where practicable. It is essential that all steam ooils be
completely free from even minute leaks since this will intro duce water into the product.
The steam colls may be introduced as "hair-pin" coils
through a manhole at the side and bottom of the tank, or as
is most often done, inserted through the manhole at the top
of the tank and then located near the bottom.
External heating coils located in the Jacket of the tank
may be used but this construction.is more expensive and less
efficient than the internal ooils.
The storage tanks may be fitted with a stirrer, either
through the top, side, or bottom of the tank and the propeller
blade Bhould be located near the bottom of the tank. However,
insertion of a stirrer through the side offers possible source of a leak and since these materials are homogeneous, it is not essential to provide such agitation for the purpose of
mixing.
-16-
0ZS31`>I
TOWOLDMON0028601 WATER_PCB-00013070
Adequate circulation can also be aooompllshed by using
a centrifugal type pump. Gear pumps or other equipment
where wear or chipping of metal parts may Introduce contam
ination should not be used. The pumps must be of the type
designed to handle hot oil. All wetted pump parts should
be either stainless steel or bronze. The oentrlfugal pumps
must be provided with a deep stuffing box and proper packing
used, as described in Chapter 3. As examples of pumps found
completely satisfactory for this Bervice, reference Is made
to Worthington Worthlte pumps. Blaokmer pumps. Dean Bros.,
Peerless and Dayton Dowd Type C pumps for handling hot oil.
Also, a very satisfactory arrangement for mixing or
circulating and pumping the fluid from the storage tank Is
to use a vertical sump pump such as a Taber pump.
All storage tanks must be amply provided with a dehu-
midlfying breather such as soda lime, activated alumina,
etc., units. This is essential to prevent moist air from
coming In contact with the dielectric. A moisture content
above 35 ppm adversely affects the eleotrloal resistivity
of these products. Provision should be made to preclude
possible leakage of the drier material back Into the storage
tank and the drier should be Inspected periodically to make
Asure that It is open and not plugged.
+0 provide ''me'uhft free" sfor*e.
B. Detailed Description
7
be a n'ltroaen blanketing system.
Drawing No. 9C-8170 shows the detailed construction of a
horizontal 15,000 gallon storage tank for Aroolor and Its
mixtures which has been found completely satisfactory.
-17-
0263146
|
TOWOLDMON0028602 WATER_PCB-00013071
The various nozzles on this tank are used as follows considering them In order from left to right on the drawing*
3" nozzle
Inlet for reciroulatlon
24" nozzle
For future agitator if required (not used)
3" nozzle
For soda lime or calcium chloride breather connection.
36" manhole
For inspection, etc. The float
guage is located in the center of this manhole.
3" nozzle
Not used.
24" nozzle
For future agitator if required (not used)
3" nozzle
Not used.
3" nozzle
Filling inlet connection.
18" x 26" Oval nozzle
For sump pump
3" nozzle
For thermometer well (see detail)
The two 24" nozzles were originally installed for installa
tion of agitators, if required. However, it has been found
unnecessary to use agitators in the storage tanks, and these
nozzles could be omitted.
It has been'found that circulation of the fluid by the sump
pump, and into the nozzle, at the opposite end of the tank, for
several hours gives satisfactory blending of the tank contents.
For pumping the dielectric from the Btorage tank, a Taber
Pump Company all bronze 2-1/2" x 2" vertical sump pump with
monel shaft has been found to be quite satisfactory for the appli cation .
18 02b3l`1`3
TOWOLDMON0028603 WATER PCB-00013072
The liquid level gauge used in the storage must be gas-tight, The storage tanks are equipped with Vapor Reoovery Systems Co.'s "Varec", gas-tight, automatic tank gauge as shown by drawing No. 9C-8278.
The storage tanks should be provided with an operating plat form suitable to the customer's conditions of operation.
The dehumidifying units used as breathers on the storage tanks can be constructed as shown by Drawing No. 9C-8248. The upper portion of the chamber is charged with anhydrous soda lime or another drying agent. Periodic inspection of the drying agent will show the formation of a cake of damp material on top about 1 to 1-1/2 inches deep. This cake should be removed and fresh material recharged. Any suitable construction similar to that shown on Drawing No. 9C-8248 may be used for the breather units.
Drawing No. D-13362 shows design detail of a 15,000 gallon vertical storage tank. The vertical type tank would seem especi ally desirable when insufficient space is available to accomodate the horizontal type tank.
0?63150
|
TOWOLDMON0028604 WATEFLPCB-00013073
CHAPTER 3
GASKETING AND PUMP PACKING
Aroclors and their mixtures soften and swell natural
rubber and many of the synthetlo "rubber" materials. Such
material not recommended for use Include, Hycar P, Koroseal,
Perbunan, Neoprene, etc. These materials are known sources
of contamination.
SUGGESTED TYPES OP PACKING AND GASKETING MATERIALS
INCLUDE:
1. For Welded Flanged Pipe Connections: Garlook Packing Co., No. 901 or No. 7021, 1/8 Inch asbestos fiber sheet. A ring of thin aluminum drawn tightly at
the flange connections may be used satisfactorily also.
2. For Pumps: Oarlock No. 234, No. 431, and Cheveron No. 7050-C are satisfactory packings. Likewise,
Durametalllo's spiral asbestos fiber may be used. Johns-Manvllle and others have comparable packing materials.
3. For Valves: Garlock No. 117 braided paoking or Its equivalent Is suggested.
4. Other Resistant Materials: It Is Indicated that duPont's Teflon, poly tetrafluoroethylene Is not attacked by hot (130C.) Aroolor and Is to be recom mended as a gasket material. Dow-Corning's Silastic, Silicone 180, Is very resistant to Aroclor and Is suggested for gasket purposes.
5. In some cases oork Impregnated under pressure with Chrysler's Cyoloweld 55-9 or Armstrong Cork Co.'s 1162-J and oured at 170C. may be used as a gaBket
material. These are baked phenollo type coatings.
6. Pipe Thread Compounds: When necessary to use pipe thread compounds, the following should be satisfac
tory If care Is taken to prevent the pipe compound from getting on the InBide of the pipe.
(a) Plastio Lead Seal - manufactured by Durametallic Corporation
(b) Ordinary white lead -20-
ozbJ151
TOWOLDMON0028605 WATER_PCB-00013074
Usually It Is not necessary to use pipe thread compounds since all screwed pipe fittings should be sealed by back brazing.
7. All new lines and fittings should be cleaned thoroughly by Bteamlng (for two hours) and dried with air or heat.
GASKETS FOR ASKAREL CAPACITORS AND TRANSFORMERS
1. For small capacitors requiring ring seals on the terminals, properly selected Silastic (silicone) tubing Is cut to make the ring gasket.
-
2. The most effective and trouble free seal for transformer lids or covers is to weld the cover onto the transformer shell. To remove the welded cover a weld cutting tool or bar Is used.
3. Cork - Nitrile rubber composition gaskets are sometimes used to combine the desired flow limiting property of cork with the resiliency of nitrile rubber. Only fine grained cork should be used In making this composition gasket. Special gasket cementing compounds such as GE's No. 1276 or No. 880 are used to coat the gaskets to further seal them against the transformer fluid and to accomplish firm bonding to the metal surfaoe.
4. Nitrile rubber gaskets are also used and require no adhesive to make a liquid-tight seal. Exposure of nitrile rubber gaskets to transformer askarel should be kept at a minimum and the gasket should not be compressed beyond 2/3 of the original thick ness .
After long time exposure to transformer askarel
fluid or its vapor, nitrile rubber is measurably
deteriorated. While gaskets made of silicone or Teflon are not attacked, these materials are relatively expensive for use In large Blzes.
Accordingly, for the most efficient performance It is suggested that welded covers be used on askarel transformers.
5. Instruments, such as temperature gauges, etc. may
be attached to the transformer using flange con
nection to pipe located below the liquid level of
the fluid In the transformer. Such flange con
nections are usually not large In diameter.
Accordingly, it seems practical to use Teflon or
Silastic gaskets to make these seals, especially
since it is known that askarel can migrate thru
cork or composition cork gaskets used under the
liquid level.
-21-
0263152
TOWOLDMON0028606 WATER_PCB-00013075
Another satisfactory approach used is to machine the flange surfaces of this type connection. Then a Spiritalllc gasket made of stainless steel ring with asbestos inter liner for resiliency can be used satisfactorily.
Screwed pipe fittings on askarel transformers require thorough cleaning of the threads to remove oil, grease and dirt. Then the threads are coated with a compound such as GE's No. 880 and then tightened.
-21A-
0263153
TOWOLDMON0028607 WATER_PCB-00013076
CHAPTER 4 SAMPLING METHODS
1.) The ASTM Standard Method for sampling electrical Insulating oils is described in ASTM Designation: D923-^9. This describes glass and metal thlefs for sampling drums, cans, and tankcars. A specially designed thief or bomb for sampling tankcars is described, also, A very good Instrument of this type is the stainless-steel Bacon Bomb Thief with which samples of the liquid can be drawn from any level of the tankcar.
The ASTM procedure describes sample containers, their cleaning and storage.
Under general precautions, the ASTM mentions that, "Samples of the fluid shall not be taken until the oil Is at least as warm as the surrounding air, because cold oil may condense enough moisture from a humid atmosphere to affect seriously its insulation properties. (In the case of tankcar lots, on some occasions there may be no choice, as it may be necessary to procure samples from a tankcar when the temperature is not above the surrounding air. On such occasions, the temperatur of oil and air also the humidity if possible, should be noted in the report of test results.) It is undesirable to do any sampling when the relative humidity of the atmosphere exceeds 75 percent, and samples shall never be taken in the rain".
-22
0
|
TOWOLDMON0028608 WATER_PCB-00013077
Several electrical manufacturers using Aroclor dielectrics, switch the tankcarB directly into the plant building or under roof before sampling and unloading.
These precautions in handling are taken to avoid any contamination of the fluids which are manufactured under very strict specifications. For example, the specificaticn for ionizable chlorides allows no detectable amount, (less than 0.10 parts per million). Moisture may not exceed 20 to 35 parts per million.
Tankcars are cleaned and prepared under close inspection before they are filled. When filled, and analysis shows the material in the car to be satisfactory, the car is then sealed with a standard railroad wire and seal inserted through the slots of the dome fittings.
Likewise, after the tankcars have been unloaded in the industry, it is requested that the dome fittings should be sealed with a railroad wire and seal.
2.) Monsanto Methods used for sampling tankcars differ somewhat from the ASTM procedure. The modified techniques are used because of their greater simplicity and they have beep entirely satisfactory as employed over many years.
A sample is never taken when it is raining or snowing, or when there is any ohance of contaminated atmosphere moving in the direction of the car. However, in case of an emergency during inclement weather, a canopy is placed over
-23-
02631S5
|
TOWOLDMON0028609 WATER_PCB-00013078
the oar dome before sampling.
A satisfactory sample bottle Is a five pint, round
amber glass, packer type container fitted with a 38 millimeter
Bakelite screw cap with an aluminum or tin cup liner. Bottles
of this description can be purchased from the Northwestern
Bottle Company, 3144 North Broadway, St. Louis, Missouri
according to their No. A-7253.
Only new bottles and caps are used. When a shipment of
bottles is received, the bottles are capped Immediately and
stored in their receiving cartons. Prior to use, the exterior
of the bottles is wiped with a clean cloth.
The simplest sampling device used is a clean stainless
steel or aluminum dipper. However, this is not a generally
preferred device because it permits sampling the oar from the
near surface, only.
The sampling device commonly used consists of a stainless
steel tube, seven feet long with one end bent into a hook, to
serve as a handle and on the other end there is a stainless
steel bucket with a perforated bottom. This bucket is about
5-1/4 inches inside diameter and 6 Inches deep to hold the
five pint bottle.
This bottle is held firmly by a stainless steel collar
made to slide along the shaft of the sampling device. This
collar haB a clamp attachment for fixing it tightly into place
where desired around the neck of the bottle.
When a car is to be sampled, a new sample bottle is
clamped firmly in the bucket.
-24-
0263^b
TOWOLDMON0028610 WATER_PCB-00013079
All dirt Is brushed and wiped away from the car dome area using a clean rag.
The car dome is opened and the cap is then removed from the sample bottle.
The sampling device is inserted into the car so that the neck of the bottle is at least twelve to eighteen inches
proper' y below the surface of the fluid. The sample taken is^discarded as its purpose is to rinse the bottle. A portion of the sample is used to rinse the interior of the bottle cap.
This procedure is repeated until a minimum of three rinses haB been made; each time the sample taken is not put back into
property the car. These rinses should be*dlscarded.
Then the sample is taken and the cap of the bottle is screwed down tightly.
When the sample has been obtained, the car dome is replaced, immediately.
The exterior of the sample bottle is wiped with a clean cloth and when returned to the laboratory it is further cleaned with a cloth dampened with pure trichlorobenzene. If the sample is to be shipped, the cap is taped with Scotch Tape.
The sampling device is also cleaned with pure trichloro benzene and Is stored in a dust free, air conditioned room.
3.) Drum Sampling! A glass thief, thoroughly cleaned with pure trichlorobenzene and dried is used to sample drums.
-25-
0263157
|
TOWOLDMON0028611 WATER_PCB-00013080
CHAPTER 5 LABORATORY ANALYSIS AND PROCEDURE FOR TREATING AR0CL0R3 AND THEIR MIXTURES WITH EARTH
A sample of the Aroolor or Aroclor mixture taken from the tankoar, or drums, as described In Chapter 4, Is analyzed In the laboratory to determine Its quality In accordance with the property values given In Chapter 7
For capacitor use, usually the Important properties tested are resistivity, power factor, chlorides, and moisture. For transformer use dielectric strength, resistivity, moisture and chlorides are the important properties.
If the sample is out of line with the shipping specifica tions, It Is Indicated that the sample ha3 become contaminated. In this case, another sample Is to be taken and the properties redetermined. If still out of specifications, the sample should be given treatment with earth.
Treatment of the dielectric with conditioned Attapulgus earth will bring the electrical properties to the maximum attainable values. While there Is complete agreement on the benefits derived from treating with conditioned earth, there Is difference of opinion on details of the method, arising from factors such as the following. No doubt, there are differences in the absorbent power of various typeB of diatomaceous earth with respect to removing moisture, impurities and additives such as stabilizers or scavengers from the dielectric
-26-
0263158
TOWOLDMON0028612 WATER_PCB-00013081
materials. The size of the earth particles, temperature and conditions of activation of the earth, the concentrations used and the temperature, the degree of agitation and time interval at which the dielectric Is given earth treatment are all possible variables which are still being studied In various laboratories.
The method used by Monsanto for treating the fluid with activated earth In the laboratory is:
The absorbent is minus 200 mesh Attapulgus* earth acti vated Just prior to use by heating in shallow trays for four hours at 400C. (752F.) or for at least twelve hours at 250C. (482F.).
At least one quart of the dielectric sample Is placed Into a clean two liter Pyrex beaker or three necked flask. The beaker or flask should be cleaned Just prior to use in a manner similar to the procedure described in Chapter 6, Method No. 11,751, "procedure for Cleaning of Electrodes, G.E. Cell and Accessories".
The flask or beaker Is fitted with a glass or stainless steel agitator. Heat Is applied using either a hot plate or a Glas-Col mantle and is controlled by a thermostat such as a Fenwal thermo switch with a stainless steel sheath.
About 0.1 to 0.2$ of the activated earth, based on the weight of the liquid is added.
#Attapulgus Division, Minerals & Chemicals Corp. of America, 210 West Washington Square, Philadelphia 5, Pennsylvania
TOWOLDMON0028613 WATER_PCB-00013082
The more viscous dielectrics such as Aroclors 1248 and 1254 are heated at about 70 to 80C. (158 - 176F.) and the less viscous materials such as Aroclor 1242 and Pyranols 1481, 1467, and 1470 are heated at about 50 to 60C. (122 to 140F.) .
After heating and stirring the sample for about four hours, It is filtered using a clean Pyrex glass suction fla3k and a Buchner funnel fitted with a Whatman No. 1 or No. 3 filter paper. This apparatus and the bottle into which the treated sample of dielectric is transferred should have been cleaned in a manner similar to the cleaning procedure des cribed in Chapter 6.
The earth treated and "up-graded" sample is then ready for final analysis of its electrical properties.
-28-
0
TOWOLDMON0028614 WATER_PCB-00013083
CHAPTER 6 TEST PROCEDURES
A. General Information
The Monsanto test methods described here with the special
equipment used are some of the control tests employed to maintain
the quality of Aroclors for dielectric use. They are suggested
as a guide for test work needed to Indicate the quality of the
dielectrics used in the manufacture of electrical goods.
The most significant electrical tests made on Aroclors for
capacitors are:
1. Dielectric constant.
2. Power Factor.
3. Resistivity.
For transformer use the most significant electrical tests
of Aroclor mixtures are:
1. Dielectric Strength
2. Resistivity.
Other than electrical tests, significant measurements of
quality include, moisture, chlorides, thermal and chemical
stability.
The following terms are defined: Dielectric Constant;
0Zfc3ibl
The dielectric constant (sometimes called specific inductive
capacity) of any substance is equal to the ratio of the capa
citance of a condenser when that substance is used as the dielectric
to the capacitance when there is a vacuum between the conductors
(for all practical purposes air at ordinary pressures may be used
Instead of a vacuum).
.50-
TOWOLDMON0028615 WATEFLPCB-00013084
Dielectric Strength:
Dielectric strength Is the rupturing strength of an
insulating material when subjected to voltage stress under
specific conditions and expressed in kilovolts. Breakdown
varies with the shape of the electrodes and does not increase
directly in proportion to the thickness of the dieleotrlc.
Power Factor:
The power factor of a dielectric is the ratio of the energy
Iobb in the dielectric to the "apparent power" in the dielectric.
Resistivity:
Resistivity is electrical resistance offered to the passage
of a steady current. The volume resistivity in ohms-centimeter
of an oil is the ratio of the d-c potential gradient in volts
per centimeter paralleling the current flow within the sample,
to the current density in amperes per square centimeter at a
given instant of time and under prescribed conditions, volume
resistivity is expressed in ohm-cm.
The analytical procedures described in detail Include:
1. METHOD NO. 11,751, "PROCEDURE FOR CLEANING OF ELECTRODES , G.E. CELL AND ACCESSORIES."
2.
METHOD FACTOR.
NH O.
11,608,
"DIELECTRIC CONSTANT AND POWER
3. METHOD NO. 11,605, "DIELECTRIC STRENGTH." 4. METHOD NO. 11,607, "RESISTIVITY. "
5. METHOD NO. 10,126, "CORROSION AND CHEMICAL STABILITY 6. METHOD NO. 10,118, "INORGANIC CHLORIDES."
7. METHOD NO. 10,087, "ACID NUMBER." 8. METHOD (MODIFIED) NO. 10,620, "MOISTURE (WATER)."
-30-
OZbSlb?
|
TOWOLDMON0028616 WATER_PCB-00013085
9. Hydrolysis Stability Test.
10. Thermal Stability Test.
Detailed Instruction and Testing Methods.
1. METHOD NO. 11,751. "PROCEDURE FOR CLEANING OF ELEC TRODES, G.E. "
Cell and Accessories.
a. The Electrode Cleaning Procedure:
1) Place the electrodes in hot electrical grade Trichlorobenzene for ten minutes.
2) Wash with unheated TCB.
3) Rinse twice with methanol and twice with tap water.
4) Place the electrodes in hot 10^ Trl Sodium Phosphate solution. Soak and heat for ten minutes.
5) Wash thoroughly with tap water.
CAUTION: After Step 5 -- DO NOT TOUCH THE ELECTRODES WITH HANDS!
6) Wash with distilled water twice.
7) Dry In drying oven for at least two hours at 120 C.
b. The G.E. Cell Cleaning:
1) Reclean the cell before use, when more than 8 hours have elapsed since the previous cleaning.
2) Follow the procedure for the electrodes starting at Step 4.
c. Cleaning of the Accessories:
1) Apply the same cleaning procedure as given for the electrodes (Steps 1 to 7) to prepare the glass spacer and beaker for next test.
2) Clean the thermometer In the same manner as the electrodes, except for Step 7.
3) Place the wet thermometer (after Step 6) directly In position In the temperature Heating Unit (Modified Fisher Isotemp Oven) and allow to dry.
TOWOLDMON0028617 WATER_PCB-00013086
OZ631<>3
2. METHOD NO. 11,608. "DIELECTRIC CONSTANT AND POWER FACTOR,
I. Apparatus
A. Oscilloscope: Heathkit Model 0-6.
B. Constant Temperature Heating Unit: Fisher Isotemp oven. Model 13-245A, modified to include inter wall connectors.
C. A. C. Generator: General Radio Type 1302-A
D. Amplifier and Null Detector: General Radio type 1231-B with type 1261-A power supply.
E. Capacitance Bridge: General Radio Co. Capacitance Bridge type 716-C.
F. Test cells: G. E. type, concentric cylinder electrodes Catalog #1,559,663. (G.E., Pittsfield. Mass. Transformer Lab.)
G. Class B driver transformer: This is used for 60 cycle measurements to excite the bridge directly from the domestic power line. It has 50 volts output with a 4800 ohm resistor in service.
H. Tuned Circuit Filters: General Radio Type 1231-P2 (400 and 1000 cycle) and 1231-P3 (60 cycle). These
filters aid in obtaining a more accurate frequency for the measurements by removing harmonics, noise, hum, etc.
II. Adjustment of Controls on Electrical Appartus
A. On Panel No. 1 (Top Panel, Amplifier and Null
Detector)
a. Turn the 4-way (main power) switch on the upper right hand side to the #3 position to determine the Dielectric Constant at 1000 cycles. Turn this switch to the #2 position for measurements at~~5U cycles
b. Allow the equipment to warm up 10 minutes.
c. Turn "GAIN CONTROL" to 6.
d. Depress "INPUT 0.03V." button.
0263164
B. On Panel No. 2 (Oscilloscope)
a. Turn "TNTEN." to about the 12 o'clock position.
CAUTION:
Do not allow a high intensity spot to remain stationary on the screen for any length of time.
-32-
TOWOLDMON0028618
WATER_PCB-00013087
b. Using "HOR. POSITION" and "VERT, POSITION controls center the image on the aoreen.
,c Adjust "FOCUS" for Bharp line.
d. Turn "FREQ. SELECTOR" to LOOKC.
.e Turn "FREQ. VERNIER" to 80. .f Turn "VERTICAL GAIN" to 5.
g. Turn "VERTICAL INPUT" to "10 VOLT MAX.". h. Turn "HORIZONTAL GAIN" to about 20.
.1 Turn "SYNCHORONIZING" to + 20.
J. Turn "SYN." to "EXT. SYN." k. Turn "GEN." to "SWEEP GEN."
On Panel No. 3 (Capacitance Bridge)
a. Turn "RANGE SELECTOR" switch to "100 C" for 60 cycle measurements and to "1 KC" for 1000 cycle measurements.
b. Turn "METHOD SWITCH" to direct.
c. Turn "DISSIPATION FACTOR" selector switch to "0".
D. On Panel No. 4 (oscillator)
a. Disregard this panel for measurements at 60 cycles.
b. On 1000 cycle measurements, depress the No. 10 "MULTIPLY BY" button.
C. Set "FREQUENCY DIAL" to 100.
d. Turn "OUTPUT" dial so that pointer is at the end of the arrow.
e. Depress the "UNBAL. 5000 OHMS" button.
When all of the above adjustments are made, the electrical
apparatus is ready for measurement of Dielectric Constant and
Power Factor.
-33-
0263165
TOWOLDMON0028619 WATER_PCB-00013088
Ill. Determination of Constants for the Apparatus
1. Carefully assemble the cell which has been cleaned and dried within the last 8 hours. Refer to Method
No. 11,751 for the procedure to use In cleaning the cells"
2. Place the cell assembly in the Fisher oven which has been adjusted to 25C.
3. Connect the back wire Inside the oven to the lead on the Inner cylinder of the cell and the front wire to the lead on the outer cylinder of the cell.
4. Connect the cable from the capacitance bridge to the terminals on top of the oven so that the inner wire of the cable goes to the back terminal and the outside mesh casing of the cable (the ground) goes to the front terminal.
5. Remove the thermometer from the top of the oven before going on with the test. hlsTs Important.
6. Make all adjustments on the electrical apparatus as directed in Pai*t I of this method.
7. Balance the bridge by rotating the "CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscilllscope is adjusted to a minimum width.
8. Record the sum of the readings on the "CAPACITANCE" dial and vernier and call this value A.
9. Remove the beaker containing the cell from the oven and fill it with C.P. benzene to a level 0.737 inches (ca. 3/4 inch) above the top of the concentric cylin ders of the cell.
10. Adjust the temperature of the benzene to 25C. while stirring with a thermometer.
11. Replace the cell in the oven (at 25C.) and make the same electrical connections as In Steps 3 and 4. DO NOT interchange connections.
12. Balance the bridge again as in Step 7.
13. Record the sum of the readings on the "CAPACITANCE"
^
dial and vernier and call this value B.
-*
-- <T\
,*
14. Calculate the cell constant by the following equation; ~
Cell Constant, K - B
- A (this is usually
.27 - 1.0 around 70 mmfd.)
" TOWOLDMON0028620 WATER_PCB-00013089
15. Remove the cell from the oven and balance the bridge as in Step 7 with the "CAPACITANCE" and "DISSIPATION" "FACTOR" dials.
16. Record the sum of the readings on the "CAPACITANCE"
dial and vernier and call this value F. (capacitance
of connecting cable.)
-
17. Calculate the CELL LEAD CAPACITANCE by the following equation.
CELL LEAD CAPACITANCE, 0 . A - F - K (this is usually around
3 mmfd.)
WHERE:
A - CAPACITANCE OF ENTIRE SYSTEM IN AIR (SYSTEM CONSTANT)
0 = CAPACITANCE OF THE CELL LEADS (CELL LEAD CONSTANT)
F = CAPACITANCE OF CABLE AND WIRES WHICH CONNECT
THE CELL AND CELL LEADS TO THE BRIDGE. (CONNECTOR CONSTANT)
K = CAPACITANCE OF THE CELL ALONE (THE CELL CONSTANT)
Tabulate the Bystem Constant (A), the Cell Lead Constant (G), the Connector Constant (F), and the Cell Constant (K) on a piece of stiff paper and post them near the instru ment where they can be easily referred to for comparison and calculations.
These constants must be checked at least once every three monthB and in all caseB where the Dielectric Constant and/or Power Factor are out of specification.
IV. Measurement of Dielectric Constant and Power Factor on Rroclors, PyranolB, Inerteens. and Trl-fetrachloro- ' benzene BlendsT
A. Test Run on Cell to Determine whether it is Clean and properly Aligned.'
1. Carefully assemble a cell which has been cleaned and dried within the past 8 hours.
NOTE: Refer to method No. 11,751 for procedure to use In cleaning cells.
0263167
5I
TOWOLDMON0028621
WATER_PCB-00013090
2. Adjust the oven control to hold at a temperature of 100C. for all materials except Tri-Tetra Blends. If a Tri-Tetra blend is to be tested, adjust the oven to hold a temperature of 25C.
3. Place the empty cell assembly in the oven and connect the back wire inside the oven to the lead on the inner cylinder of the cell, and connect the other (front) wire to the lead on the outer cylinder.
4. Connect the cables from the capacitance bridge to the terminals on top of the oven so that the inner wire of the cable goes to the back terminal and the outside metal casing (ground) goes to the front terminal.
5. Allow 15 minutes for the cell to reach temperature equilibrium inside the oven.
6. Remove the thermometer from the top of the oven before taking any measurements on the bridge. This is important.
7. Make all the adjustments on the electrical apparatus as directed in Part I of this method.
8. Balance the bridge by rotating the "CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscilloscope screen is adjusted to a minimum width.
9. Record the sum of the readings on the "CAPACITANCE" dial and vernier and compare this value with the SYSTEM CONSTANT determined in Part II of this method.
IMPORTANT: If the value obtained in Step 9 does not agree with the System Constant A (Part II) within 5 uuf, the cell must be re-cleaned, re-dried, re-assembled, and the test run for the System Constant must be repeated.
NOTE: Although the above test run must be made prior to each analysis, the value obtained in Step 9 Is not to be used in calculations but is to be used only as a check on the cleanliness and alignment of the cell.
-36-
02b31ba
|
TOWOLDMON0028622 WATER_PCB-00013091
B. Procedure for Testing Materials
10. Remove the cell from the oven and fill the beaker
with the material to be tested to a level 0.737 inches (ca 3/4 Inch) above the cylinders of the cell.
11. Adjust the temperature of the sample to 100C. (use hot plate; for all materials except Tri-Tetra blends. For Tri-Tetra blends, adjust the tempera ture of the sample to 250. using an ice-water bath if necessary.
NOTE: Stir sample continuously with a thermometer while adjusting the temperature.
12. Place the cell and sample in the oven and make the same connections from the cell to the bridge as in Steps 3 and 4. DO NOT interchange connec tions .
13. Allow 15 minutes for the cell to reach temperature equilibrium inside the oven.
14. Remove thermometer from the oven before taking a measurement. (This 1b important.
15. Make the adjustment of controls on the electrical apparatus as directed in Part I of this method.
16. Balance the bridge by rotating the "CAPACITANCE" and "DISSIPATION FACTOR" dials on Panel No. 3 until the wide vertical band on the oscilloscope screen is adjusted to a minimum width.
17. Record the sum of the readings on the "CAPACITANCE" dial and vernier, and call this value X.
18. Record the sum of the readings on the "DISSIPATION FACTOR" dial and switch. Call this value D.
Calculations :
Dielectric Constant =
X-F-Q ------- K-------
Where:
X Capacitance reading from Step 17. F a Connector Constant (Determined in Part II) 0 a Cell Lead Constant (Determined in Part II) K a Cell Constant (Determined in Part II)
02h31<>q
|
TOWOLDMON0028623 WATER_PCB-00013092
% Power Factor = f x D
Where:
f = Test Frequency (60 cycles or 1000 cycles) f0= Frequency of "Range Selector" on Panel No.3 D = Dissipation Factor reading from Step'l8.
NOTE:
When D (dissipation factor) Is less than 0.1, the dissipation and power factors differ oy less than 0.0005. Therefore, for our measure ments, power factors and dissipation factors are equal.
Precision: (Reference: General Radio Manual for Model 716-C Capacitance Bridge)
a. Capacitance readings are precise to + 2 mmfd. x mul tiplier reading (+ 0.2$ of full scale for each range) when the dissipation factor is less than 0.01.
b. Dissipation Factor (Power Factor) readings are pre cise to + 0.0005 or + 2$ of the dial reading which ever is Targer, for values less than 0.1 for D (Dissipation Factor).
METHOD NO. 11,605, "DIELECTRIC STRENGTH."
a. Apparatus and General Information
The electrical equipment necessary to provide high
voltage to permit the determination of dielectric
strength of liquid dielectric at commercial power
frequencies is basically quite simple.
The equipment assembled in the laboratory consists of a high voltage transformer of good design and with a current capacity of 2.43 KVA and with equip ment for control of the voltage and a means of measuring the voltage and to provide safety for the operator.
-38-
0 6 3170
TOWOLDMON0028624 WATER_PCB-00013093
It is enclosed in a steel gray crackle finished
cabinet measuring 42" high, 22" wide, 17" deep
and set on truck casters for easy mobility.
Protective equipment incorporated in this apparatus
prevents the application of high voltage unless all
safeguards are complied with. The door on rear of
cabinet must be closed. The cover over the oil
must be all the way down and the voltage control
must be at 0 position. Failure to comply with these
requirements will prevent any action when the red
button Is depressed.
The test cup; Transformers, VoltmeterB, and Accessories
The aBkarel testing cup type No. 224809 supplied by
General Electric Company is mounted on the top
rear of the cabinet. It is protected by a heavy
plastic cover, hinged at the rear for accessibility
to the receptical.
It is equipped with safety contactor so placed that
the circuit energizing the high voltage contactor
cannot be completed unless the protective cover is
completely lowered and in place. It is impossible
for the operator or anyone elBe to touch the testing
cup when high voltage is applied.
The High Voltage Transformer manufactured by the
Kelly-Koett Manufacturing Co. is of the closed core,
oil immersed, Bhell type design. Rate @ 81,000 volt
@ 40 mlllampers. It was recovered from a used X-ray
machine purchased quite inexpensively.
I
TOWOLDMON0028625
WATER_PCB-00013094
An auto transformer from the same X-ray machine is connected so as to limit the out-put voltage of the high voltage secondary to 50,000 volts.
The primary of the auto transformer is connected to the secondary of a 2-1/2 KVA powerstat variable auto transformer supplied by the Superior Electric Company.
Power to the powerstat is controlled by a 4 con tact 30 amp. solenoid circuit breaker.
The voltmeter mounted on top near front edge is connected across the powerstat secondary and is calibrated to read directly in Kilovolts in the range of 0 - 50 K.V.
The overload circuit breaker consists of a small relay connected between one side of the high voltage transformer secondary center tap and ground. It is adjusted to break contact on a current drain of about 50 mllliampers. The circuit for the coil of the solenoid circuit breaker is wired through the contacts of this relay.
-40-
0263172
TOWOLDMON0028626 WATER_PCB-00013095
Safety and Operating Controls
1) Door Interlock switch located on rear door.
2) Test cup cover Interlock switch.
3) Powerstat switch mounted on rear of unit arranged so that high voltage contactor cannot be closed unless powerstat Is at zero position.
4) Main power switch, on front panel.
5) Powerstat voltage control on front panel.
6) High voltage contactor push button on front panel (red).
T) Signal lamps mounted on top around voltmeter. Purpose and operation described in method of use.
Procedure
1) Ascertain that the temperature of the material under test Is 25 ( 0.5)"C,
NOTE: Testing at other temperature Is likely to give variable results which may be misleading.
2) Shake the sample container so as to thoroughly mix the askarel before filling the test cup.
NOTE: This operation is especially important with used Aroclor as the impurities may settle to the bottom and the test may be misleading.
3) Rinse the testing cup three times with Bmall portions of the sample to be tested.
4) Immediately after final rinse, fill the cup to a height of not less than 20 mm. (0.787 in.) above the top of the electrodes.
5) Rock the cup a few times in order that any entrapped air may escape. Close cover over oil test cup.
6) Allow to stand 3 minutes. CAUTION: THIS IS IMPORTANT.
7. Turn main toggle switch on front panel to "ON" (or up) position. Both green and amber pilot lights on the top at either side of the voltmeter will now glow. 0263173
TOWOLDMON0028627 WATER_PCB-00013096
NOTE: The green signal light is connected across the
115 volt in-put and denotes that line voltage has been applied to operating control circuit.
Amber light is connected in series with sensitive switoh located under high voltage contactors and connected to its armature. It indicates that high voltage contactor is in ltB rest position and away from contacts energizing auto transformer.
8) Turn voltage control (large knob on front) to extreme counter-clockwise position.
9) Depress red button on front. ThiB energizes high voltage transformer and circuit breaker
and is indicated by amber light going out and the red light directly over voltmeter will lights
10) watch the voltmeter and, while holding the button "IN", turn the voltage control at such speed that will cause voltage as indicated on voltmeter to rise at a rate of 3 K.V. per second.
11) Note and Record the voltmeter reading at break-
33wn.
------------
12) Repeat the test until two successive breakdowns ocour on each of two fillings of the test cup which do not differ by more than 10$.
Report the average value of these two readings (Step 12) as the Dielectric Strength. If the limit of the instrument is reached before breakdown, report the Dielectric Strength as 50 K.V. at 25C.
Cleaning of the test oupi After the test is completed, drain the cup. Plush the cup with benzene. Then fill with Aroclor 3248 and let stand, until the next analysis.
-42-
0?61174
I
TOWOLDMON0028628 WATER_PCB-00013097
NOTE: An exception, when samples of oil from the plant are brought In for test, the cup must be thoroughly cleaned with benzene and carbon tetrachloride before and after running the test The electrodes:
The testing cup has two electrodes. Both electrodes are movable and have twenty threads to the Inch with index notches on both the electrodes and the lock nuts. To set the flap: Arrange one of the electrodes and the look nuts with the index marks in line. Move the other elec trode until it comes in firm contact with the first electrode and lock it. Now unscrew the electrode with the index marks in line (Step 1) two complete turns and look it. This will leave a gap of 0.1 inch between faces of the electrodes. Cleaning of the electrodes and the test cup free of carbon coating: The following ASTM method of cleaning shall be followed when it is apparent from visual inspection that the electrode discs of the cup are coated with carbon. Wipe clean with dry calendered tissue paper the electrodes and the test cup.
TOWOLDMON0028629 WATER_PCB-00013098
CAUTION: It is important to avoid touching the electrodes with the finger or with portion of the tissue paper which has been In contact with hands. Rinse the electrodes and cup with dry lead-free gaso line, Stoddard Solvent (or dry, waterwhite Kerosene) until they are entirely clean. Care should be taken not to touch the electrodes or the inside of the cup after cleaning so as to avoid possible contamination. METHOD NO. 11,607, "RESISTIVITY." a. Apparatus:
General Radio Company Megohm Bridge Type 544-B. This is a combination of Wheatstone bridge and vacuum tube voltmeter for indicating null. The direct measurement of resistance up to 1,000,000 megohms Is made possible by the use of a vacuum tube detector which absorbs negligible amount of power. The voltage applied to the unknown resistor is held approximately constant, regardless of the value of the unknown resistance. This condition is necessary to measure resistance properly. The accuracy of the Instrument in the range en countered in the measurement of Aroclor resis tivity, 100 to 1000 megohm is + 6%.
-44-
02t3'7b
|
TOWOLDMON0028630 WATER_PCB-00013099
The instrument is equipped with a 1X5 volt AC power supply which supplies all operating voltages for the bridge indicating circuits and in addition supplies 500 V DC for application to the material under test. The Instrument is completely enclosed in a waxed finish shielded oak cabinet measuring 8-1/2" wide, 22-1/2" long and 8" high. Approximate weight--26 pounds.
Test Electrodes: Two concentric nickel cylinders with feet, obtained from General Electric Company. The inner electrode has outside diameter of 2.8" and a height of 3.25" with area of 184 sq. cm. The outer electrode has an inside diameter of 3" and a height of 3.25" with area of 198 sq. cm. The distance between electrodes is, therefore, 0.1" or 0.254 cm. By theory, electrode constant (K) area/length is 191/0.254 or 752 where average area is 191 sq. cm. Also K = 36 x 10" x C (farads with air as dielectric) or 11.29 x C (mmfd. with air as dielectric).
Glass Plate: Pyrex about 3-1/2" diameter with concentric grooves to assist in spacing electrodes. Obtained from General Electric Company.
Heating Unit; Assembled in the laboratory and is the same unit
-45-
0?63177
TOWOLDMON0028631 WATER_PCB-00013100
described In Dielectric Constant Apparatus (see
Method No. 11,608; Equipment).
Procedure:
1) Assemble the test cell. Place the recentlycleaned (within the last 8 hours--see Method No. 11,751.. Step 9) electrodes In an 800 ml. beaker.
2) Measure the capacitance of the test cell (C0) according to Method No. 11,608 (Dielectric Constant and Power Factor measurements.)
3) Fill the cell assembly until the liquid level Is 3/4 Inch above the top of the electrodes.
4) Heat the assembly on the hot plate to 100 (+ 0.5)C.
5) Place the assembly Inside of the testing oven.
6) Attach top lead (+) on the megohm bridge to inner electrode.
7) Attach other lead to outer electrode.
8) Throw the three switches at the top of the megohm bridge to "ON" position.
9) Allow 10 minutes for assembly to reach temperature equilibrium Inside the oven.
DANGER: Make sure control knob Is in "CHECK" position. Otherwise, painful shock will result if leads are
touched"
10) Bring the galvanometer pointer to zero by turn ing the "ZERO ADJUST" knob in the direction in which the pointer of the galvanometer should move.
11) Turn the control knob to "CHARGE" position for 30 seconds.
12) Turn the control knob to "OPERATE" position and return the galvanometer pointer to zero by ad justment of the "MULTIPLY BY" switch and the megohm dial.
13) Read after 30 seconds.
-46-
TOWOLDMON0028632 WATER_PCB-00013101
Calculation:
Resistivity* - Megohm dial reading (Step 12) x "Multiply By" reading (Step ll) x capacitance of cell (Step 2) in mmfd. x 11.29 x 0.001.
Report the result in units of 109 ohm-cm.
*Values of resistivity are qualified by designation
of temperature and voltage. These are for this test,
100C and 500 volts DC.
NOTE: It is important that the product under teBt, electrodes, and beaker be at uniform temperature for this determination. Temperature variations in " different parts of the sample will cause the galva nometer zero to change constantly and give misleading results.
,
CAPTION: Inasmuch as measurements must be made at a
potential of 500 volts DC a shock hazard exists in
the handling of this appartus. With the control
knob in the charge and operate position full voltage
of the bridge (500 volts) is applied to the positive
and low terminals and through the test leads to the
electrodes. Do not attempt to handle the electrodes
of the test leads unless the control knob is in the
"CHECK" position. Possible penalty for failure to
observe this precaution -- Painful Shock.
METHOD NO. 10,126 "CORROSION AND CHEMICAL STABILITY."
a. Apparatus: G.E. Corrosion Apparatus consists of the following:
1) A Corrosion Flask - It is a 300-ml. Pyrex flask
-^7-
0?61179
TOWOLDMON0028633 WATER_PCB-00013102
with a ground glass 24/40 joint equipped with
a 12-inch straight tube as an air cooled con denser. The air-condenses is painted on the outside with aluminum. '
2) The Corrosion Apparatus: A transite box. 32"
long x b" wide x 5" deep. The top of the box represents a split transite board with 5 holes cut to fit the flaBks.
'
The box is heated by two 500-watt, 15 volt G.E. Strip heaters with off-set terminals at one end (23.5" overall length).
The heating length of the heating element is covered by a copper strip 19-1/2" long x 4" wide x 1/4" thick.
The temperature is controlled by an automatic thermostat with temperature setting indicator.
Procedure:
1) Roll a rectangular (2" x 4") piece of aluminum foil so that it will pass through a ground glass 24/40 Joint of the corrosion test flask.
CAUTION: Be careful that after rolling the specimen does not touch Itself at any point.
2) Wash the aluminum foil (Step 1) scrupulously with
acetone, distilled water, acetone, benzene, and chloride-free ether.
3) Then place the foil on a clean watch-glass and dry in an oven at 110C. for 30 min. After
cleaning handle the specimen with tongs or forceps only.
4) weigh accurately on an analytical balance the specimen (Step 3) at room'temperature.
5) Drop the weighed aluminum foil into the chloridefree corrosion flask of the "O.E. Corrosion Appa
ratus." Rinse out flask with sample and rinse end of condenser with sample.
6) Add 200 ml. of the product under test to the aluminum foil (Step 4 and 5).
7) Set the corrosion flask in the corrosion test appa ratus.
-48-
OP63180
|
TOWOLDMON0028634 WATER_PCB-00013103
8) Attach a 12-inch straight-tube air-cooled condenser, the outside of which is painted with aluminum.
9) Cover the exposed part of the flask with aluminum foil.
10) Heat the flask for 6 (+ O.l) hours at 210 (+ 5)C.
The temperature of the liquid in Ihe test flask is mea sured indirectly using a thermometer inserted through a cork stopper and into similar liquid contained in an identical flask seated adjacent to the test flask on the heating chamber.
11) At the end of the heating period, detach condenser from the flask before removing-it from ^he hot plate.
12) Remove the flask from the hot plate and cover all of the flask with aluminum foil (when the flask is not on the hot plate.)
13) Without removing the aluminum foil covering of the flask, analyze the product (Step 6) remaining in the corrosion apparatus fort
a) Appearance, Color, and Condition. b) Inorganic (Free) Chlorides--Apply Method No.10,118 c) Acidity (Acid Number) - Follow Method No. 10,087
14) With a pair of clean, straight nichrome tongs, remove the aluminum foil specimen (Step 5), wash thoroughly, dry and weigh accurately on an analytical balance in the same manner as before (Steps 2, 3 and 4).
Report the corrosion as loss or gain in weight to the nearest 6.OOO1 g. and the Chemical Stability, as indicated by the analysis of the produots "After Corrosion Test", in the same way as reported for the original (as received) material.
METHOD NO. 10,118, "INORGANIC CHLORIDES."
a. Preparation of Standards;
I) Make a primary standard of 100.0 ppm by weighing 0.1648 g. C.P. NaCl into a chloride-free 1 liter volumetric flask. Dilute to the mark and mix thoroughly. Make a 10.0 ppm standard by diluting 100 ml. of the primary standard to 1 liter, and mixing well. For every 0.1 ppm standard, dilute to 10 ml. of the 10 ppm standard to one liter and
-49-
0763181
|
TOWOLDMON0028635 WATEFLPCB-00013104
mix well. A 0.1 ppm beam is considered the very
faintest beam perceptible to tne eye between 15-45 seconds after adding the A.gNGo solution, if the beam intensity is not vislbie^ar all, or if easily visible (too strong}, discard the solutions and make new standards,
2) Weigh 20.0 g. C.P. AgNO^s into a chloride free
dark bottle. Add 20 ml. C.P. HNO3 (chloridefree). Dilute to 200 ml, with wa.er.
3) All solutions should be freshly prepared every
two weeks and stored in glass-Btoppered Pyrex
bottles.
'
b. Light Source:
Employ the 2 battery Penllte flashlight, having a 3-4 mm. light aperture. New batteries must be used frequently in order to perceive beams properly.
c. Procedure:
1) Thoroughly rinse two separatory funnels with
chloride-free water three or four times. Then
take an aliquot from each funnel in a test tube
which has been rinsed with chloride-free water.
Test these aliquots for Tyndall beam3 by auding
3-5 drops of AgNOg and allowing 45 sec. for full
beam to evolve. Absolutely no dust or chloride
beam should be present. [If beam is present,
rinse all equipment with 1:1 HNOo and repeat
Step 1).
J
2) When funnels are beam-free, drain out all the water except 50 ml. In one and 25 ml. in the other. Heat the water in both funnels tc boiling. (Hold stopper while heating as steam may cause stopper to fall.)
3) Transfer 50 ml. of the sample from the sample bottle at a temperature of 95-100"C. into the separatory funnel containing the 50 ml . of
boiling water. (As a precautionary measure, pour some of-the sample from the 3ample bottle
into a waste beaker before adding the 50 ml. to the funnel.)
4) Stopper the funnel and shake vigorously for at leaBt 1 minute, venting frequently through the stopcock. (Care must be exercised at all times to touch neither the lower part of the funnel stem nor the ground part of the stopcock.)
076318?
TOWOLDMON0028636
WATER_PCB-00013105
5) Allow the layers to separate and drain off the sample Into the second funnel containing the 25 ml. of boiling water. . (As before, drain off a few ml. of the sample Into a waste beaker before draining the sample Into the second separatory funnel.) It may be necessary to heat the sample when transferring the sample to the second funnel; e.g., Aroclor 1260.
6) Repeat step 4 and allow the layers to separate. Then drain off the sample Into a waste beaker.
7) Combine both water extracts In one funnel and
shake thoroughly.
8) Take approximately a 10 ml. aliquot of the water extract out through the bottom of the funnel into a 3/4" x 6" test tube. Again, first allow a few ml. to drain out before taking the aliquot. (The test tube used should be rinsed with chloridefree water several times before using.)
9) Add approximately an equal portion of chloridefree ether. (The ether is tested by shaking a portion of it with chloride-free water and testing for Tyndall beam at the end of 45 sec. If beam is present, waah ether several times with chloridefree water until washings show no beam after adding 3-5 drops AgNOj).
10) Shake the ether-water mixture until the emulsion in the sample disappears and the water layer Is completely beam free before adding AgNOa. If emulsion is difficult to break, add sample dropwise through the ether and then shake.
11) Add 3-5 drops of 10# AgNOa solution and test for chloride beam for 45 Sbo. exactly. If no beam is present at the end of 45 seconds, report as <0.1 ppm. The very faintest of beams is considered 0.1 ppm. If beam Is stronger it will be necessary to compare with standards of 0.15, 0.20 up to 1.0 ppm, adding the 3-5 drops of AgNOa and comparing at the end of 45 sec.
The method is precise to the nearest 0.1 ppm.
Report results to the nearest 0.1 ppm.
METHOD NO. 10,087, "ACID WJltBER."
a. Reagentst
.
1) Nitration grade benzol. _51_
026318*
TOWOLDMON0028637 WATER_PCB-00013106
2) Anhydrous methanol.
3) A saturated solution of phenol red (phenol sulfonphthalein) in methanol (approx. 0.1$).
4) A 0.01 N solution of KOH in methanol.
b. Procedure:
1) Place 100 ml. of benzol, 100 ml. of methanol and 0.5 ml. (pipette) of phenol red indicator into one of two clean dry 500 ml. Erlenmeyer flasks.
. 2) Neutralize carefully with the 0.01 N KOH (to be first definite pink color.)
3) Pour the mixture back and forth between the two flasks several times. If the solution is still neutral, divide it equally between the two flasks, if not, repeat Bteps 2 and 3<
4) Weigh (+ 0.05 g.) into one of the flasks a 75.0 + 5-0 g. sample and titrate with the 0.01 N, KOH until the sample matches the blank.
c. Calculations:
Acid No. (mg. KOH/gram sample) b ml. 0.01 N KOH x 0.56 Sample Weight ^
Report the results to the nearest 0.001 if they are below 0.1, otherwise to the nearest 0.01.
The method is precise to + 0.002 for add numbers below 0.01 and to + 0.01 Tn the range of 0.1 to 0.01.
NOTE 1: To convert mg. KOH/gram to mg. NaOH/gram, multiply by 0.715.
METHOD MODIFIED NO. 10,620, "MOISTURE (WATER)".
a. Introductory Comment:
The Karl Fischer Reagent titration method used in the analytical laboratory involves use of an analyt ical balance to weigh accurately about one drop of water used in preparing the standard. Since an analytical balance may not be available, the method has been modified and uses a purchased standard water solution as described below. Also, in the laboratory a "Dead Stop" potentlometrlc method for determining
-52-
026118'.
|
TOWOLDMON0028638 WATER_PCB-00013107
the end point is often used. However, as this equipment may not be available, the procedure described below uses the visual indicator change for determining the end point.
b. Apparatus and Reagents:
1) Karl Fischer Burett, Automatic Pyrex No. 5750,
25 ml. capacity. Ace Glass Company, Vineland, New Jersey.
2) Water Standard in Methanol. No. SO-W-2 (1 ml. = 1 mg. HgO) Fisher Scientific Company, 2800 Jefferson Ave., St. Louis, Missouri.
3) Karl Flsoher Reagent Solution No. SO-K-2, Fisher Scientific Company.
o. Standardization of Karl Fischer Reagent
Into a 500 ml. clean, dry Erlenmeyer flask, place
about 100 ml. "Anhydrous" methanol (commercially
available, 99-9556). Add Karl Flsoher reagent to
this blank until the first color change from lelnon
Jellow. It is not necessary to read the burette
at this point. Carefully pipette 50 ml. of standard
water solution into the blanked methanol. Refill
the Karl Fischer burette. Titrate the solution
with gentle swirling to mix, until the same color
is obtained as was obtained for the blank. Now
read the burette.
.
Moisture value of K.F. reagent in terms of grams
HgO per ml.
. (Moisture value of
(Ml. Standard HgO solution) standard water so
lution in gm. per
_________________________
ml. stated
ml. Itarl Fischer Reagent
d. Solvent Mixture:
Since the solubility of the different askarels varies, the following solvent mixtures are suggested:
Material
Anhydrous Benzene Anhydrous Methanol
Pyranol 1478 Fyranol 1488 Pyranol 1467 Pyranol l43l Pyranol 1495 All Aroclors Inerteen PPO
0 ml. 100 ml.
100 ml. 100 ml. 100 ml. 110 ml. 100 ml.
* 'T* `
300 ml. 200 ml.
200 ml. 200 ml.
200 ml.
190 ml. 200 ml.
TOWOLDMON0028639 WATER_PCB-00013108
e. Procedure, "Visual End Point."
1) Place 100-300 ml. of dry solvent mixture (c) in a dry 500 ml. ground glass-stoppered Erlenmeyer flask.
2) Titrate the solvent with K.F, reagent to the visual endpoint, l.e., the first change from the yellow to reddish orange that persists for 30 seconds. Refill the burette.
3) Using a beam balance, weigh to the nearest 0.1 gram by difference, a sample containing 0.03 to 0.06 grams H2O into the flask.
4) Stopper and shake until the sample is in solution.
5) Titrate the solution with K.F. reagent to the endpoint described in Step 2. Record the volume of K.F. reagent used.
Calculation!
% HgO a ml. of K.F. reagent xHpO factor x 100 Sample Weight
References! Mitchell, J. and Smith, D.M., Chemical Analysis, Vol. 5, Aquametry, Intersoience Publishers, Inc., New York, (1948)
-54-
TOWOLDMON0028640 WATER_PCB-00013109
9- 'HYDROLYSIS STABILITY TEST POR AROCLOR
Purpoae
To quantitatively determine the presence of unstable chlorine compounds in chlorinated biphenyls (askarels).
Principle
The method is based upon the hydrolysis of unstable chlorine compounds in askarels by methanoiio sodium hydroxide. The resulting chloride ion is determined potentlometrlcally by titration with silver nitrate solution in an essentially nonaqueous medium. The measured chloride ion, reported as parts per million in the askarel sample, is indicative of the relative stability of the askarel in a dielectric system.
Reagents
1. Methanol (chloride free) - 5 liters of methanol are refluxed
with 0.5g Analytical Reagent Grade AgNOq for 1/2 hour. The methanol is then distilled from the AgNOq, discarding the first 100 ml. to flush the apparatus. 90# of the charge is distilled from the flask and the oontents of the flask are discarded. The methanol should be ohecked to assure purity by titration. The chloride ion concentration should be less than 0.01 ml. of 0.005N AgNOj per 100 ml. of methanol.
2. Sodium Hydroxide Reagent - Analytical Reagent Grade NaOH (may be obtained from Mallinckrodt Chemical Company) is used to prepare this reagent. A 0.1N solution is prepared by dissolving 4.0'grams
of analytical reagent grade NaOH in 1 liter of chloride free methanol.
3. Sulfuric acid - Prepared by a 50:50 volumetric dilution of Analytical Reagent Grade oonoentrated sulfuric acid (can be obtained from Malllnokrodt Chemical Company) with chloride free (deionized or distilled) water. The acid is always poured into the water with constant stirring to prevent any dangerous build-up of heat.
4. 0.005N AgN03 and 0.0025N AgNOq - Prepared by dilution of an ampoule of concentrated aqueous AgNO,. These ampoules can be obtained from Anachemica Chemical Limited, Champlain, New York.
This reagent may also be prepared by dissolving 0,8495 6- of Analytical Reagent Grade AgNQj crystals (may be obtained from Mallinckrodt Chemical Company; in one liter of chloride free water
containing 3.0 ml. of concentrated nitric acid. This solution should be standardized against a pure chloride standard. A sodium chloride crystal such as used in infrared spectrometer cells is a good source of pure NaCl. The AgN03 solutions should be checked
(at least monthly) to assure a consistent reagent.
0^63187
|
TOWOLDMON0028641 WATER_PCB-00013110
5. Acetone (chloride free) - Prepared by distillation from AgNOo as described above, for methanol and should also be checked by potentiometrlc titration to assure optimum purity. Normally a chloride content of less than 0.01 ml, of 0.0025N AgNOj per 100 ml. is derived by this method.
6. Benzene - Analytical Reagent Grade benzene Bhould be used. This material is normally chloride free but Bhould be checked by potentlometric titration to be certain. Analyti cal Reagent Grade benzene may be obtained from Mallinckrodt Chemical Co.
Equipment
1. 200 ml. tall form beaker (Berzelius type).
2. Magnetic stirrer - A suitable magnetic stirrer with ring stand base can be obtained from Fisher Scientific Co. Cat. #14-511-1. This stirrer has a built-in rheoBtat and should be set at full speed and operated through a varlac to adjust its speed. This will prevent heating of the stirrer during the stirring operation.
3. Teflon magnetic stirring bar - The bar should be cylindrical in shape and of one piece molded construction, one inch long, may be obtained from Fisher Soientlflo Co., Cat. #9-311-9.
4. Microburet graduated in 0.01 ml. divisions - A suitable buret may be obtained from Scientific Glass Apparatus Co., Inc. Bloomfield, New Jersey Cat. #JM-570.
5. Silver electrode - The Beckman silver billet electrode Cat #39261 1b the preferred type.
6. Glass electrode - A standard glass electrode suoh as Beckman electrode Cat. #40498.
7. pH meter suitable for use with glass electrode - A model GS Beckman pH meter can be used. This Instrument has the expanded scale and provides greatest sensitivity to incre mental emf changes. A somewhat less sensitive but, nonethe less, useable meter such as Beckman "Zeromatio" or the Leeds Northrup line operated pH meter can be used.
8. Water bath - An individual glass water bath 150mm in diameter 75mm high and containing 600 ml. of water heated to 40C. + 1C. is used. This glass water bath can be obtained from " Corning Glass Co., Corning, N.Y. Cat. #3140.
9. Usual laboratory glassware - 25 ml. pipette, buret or pipette graduated to deliver 0.5 ml., wash bottles for pure acetone methanol, water and a sturdy rlngstand.
ozena9
|
TOWOLDMON0028642 WATER_PCB-00013111
Procedure for 1242 Aroclor (1499 Fyranol)
1. Twenty five grama of askarel ia weighed into a tared 200 ml. beaker to the nearest 0.01 gram on a suitable balance.
2. The magnetic stirring bar ia then added to the beaker containing the sample (without the bar touching the operators'
hands).
3. Twenty five ml. 0.1N NaOH (methanolic) is added by means of a 25 ml. pipette and the beaker is covered with a watch glass.
4. The sample beaker is Immersed to a depth of 1 1/4 inches in the 40 + 1C. water bath on a magnetic stirrer and clamped securely to a firm support. The sample is stirred at as fast a speed as possible, without pronounced splashing, for 1 houf. The water bath is not heated. No effort is made to maintain the temperature at 4oC., and it will drift toward equilibrium with room temperature.
5. After the 1 hour stir, the sample beaker is removed from the bath, 0.5 ml. of dilute sulfurio acid is added to the sample by means of a suitable pipette or buret. 125 ml. of chloride free acetone is then added (a graduated cylinder is suitable for this purpose).
6. The sample is then titrated with 0.005N AgN03 solution using the silver-glass electrode system.
Normal samples of askarel require extremely small amounts of AgNOo, for this reason the titration is run using 0.01 ml. additions and allowing sufficient time for equilibrium to be established before recording the emf change. If a change of less than lmv per 0.01 ml. addition is observed for 3 or 4 .01 ml. increments, larger additions of AgNOo may be used for instance .05 ml. until such a change isJ
observed. The additions then are reduced to 0.01 ml. again to complete the titration. The endpoint normally is defined
by two 50mv changes. A normal titration would yield the following typical data.
MV .idMV* VOj dML dMV/dML X 10"2
400 0
.06 0
392 8 .07 .01
352 8 . .08 .01
341 11
.09 .01
321 20
.10 .01
271 50
.11 .01
221 50
.12 .01
201 20
.13 .01
285 16
.14 .01
0 8 8
11 20
50 50 20 16
* Using the QS pH meter the change 1b measured in 0.2mv
units and hence the meter changes observed would be 5 times this value (i.e. 25 units for 5mv).
I
I "I
" TOWOLDMON0028643 WATER_PCB-00013112
To calculate the change per 0.01 ml. observed, the mv
change Is divided by the volume of AgNOg. By plotting dmv/dml vs. ml., the endpoint may be found to the nearest 0.001 ml. This gives a sensitivity of + 0.007ppm - to define the endpoint to + .01 ml. no plotting is necessary and a sensitivity of + T5.07ppm is assumed.
7. A reagent blank is run exactly as above omitting the askarel sample.
Calculations
Subtract the reagent blank from the total volume of AgNOj and for the sample then:
Reactive Chlorine (ppm) Net Volume AgNC^XNormality AgNOgX35.46xio3 weight
Procedure for 1254 and 1260 Aroolors (more viscous askarels)
The procedure is followed exactly as above except that under Procedure, Step 2, 5 ml. of benzene is immediately added to the askarel sample and stirring bar. The sample is heated until it dissolves in the benzene and cooled to room temperature before proceeding to Step 3-
The benzene, of course, should be included in the reagent blank determination.
Procedure for Micro Test
The dechlorination test may also be run on 5 gram samples of askarels with a reduction in sensitivity. It is run exactly as the 25 gram test above except that the amount of reagents
then used are 5.01 ml. NaOH (0.1N methanolic), 0.1 ml. H0SO4 for acidification, and 50 ml. of acetone to dilute the sample. 0.0025N AgNOg is used to titrate this size sample. The sensi tivity is then + 0.l8ppm rather than + 0.07ppm given by the 25 g sample (without plotting the endpoint).
3 eneral Comment s
A rapid titration can be made to the nearest 0.1 ml. using
the normal potential at the equivalence point or use can be made of an automatic tltrator for routine control procedures. The sensitivity in either case should be within + 0.7ppm of
the value obtained by more refined techniques with 0.005N AgNOj and a 25 gram sample.
The usual analytical precautions should be exercised in using this test method to prevent cross contamination from other sources of halogen in the laboratory. This means that all glassware, apparatus, and the area in which this test is run should be analytically clean"
opbn'fo
|
TOWOLDMON0028644 WATER_PCB-00013113
10 1`THERMAL STABILITY METHOD FOR AROCLORS"
Scope
This method measures the thermal stability (chloride content) of chlorinated biphenyls used primarily as dielectrics. It Is used for determining the quality of finished Aroolors.
Principle
Certain Impurities If present in chlorinated biphenyls will
break down at elevated temperatures with the liberation of HC1. The volatile HC1 Is swept out of the sample with air, absorbed In water and titrated with silver nitrate solution. The results are expressed as parts per million chloride obtained during a 16 hour thermal stability test period.
Reagents
1. Acetone. No special grade Is required. It must contain no titratable chlorides.
2. 1# HNO3. Dilute 1 ml. concentrated HNO3 to 100 ml.
3. 0.005 NAgN03. 0.8495g to 1000 ml. 5 ml. 0.1 NAgNOo (if
available) to 100 ml.
J
Apparatus
1. Pressure Regulator. Moore - Model 40 - 2 - 0-50" Water.
Moore Products Co. H & Lycoming St., Philadelphia 24, Pennsylvania.
2. Thermoregulator. Cenoo - 99015 - (Central Scientific Co.)
3. Relay. Ebert Micrelay SPST Std. Type. Ebert Electronics
Corp., Queens Village, N.Y. (Any sensitive, reliable relay can be used).
4. Stirring Motor. Bodlne NSI-13 B-2224 1/40 HP. 1725 R.P.M.
5. Bath Fluid, Dow Corning 550. 5 gallons
6. Leeds & Northrup ac. operated pH Meter - Cat. No. 7664
7. Silver wire electrode
02fc3i<)i
8. Mercurous Sulfate Reference Electrode. Modified L & N calomel reference electrode prepared as follows. Dismantle the internal element from the salt bridge tube of a standard
L & N calomel reference electrode. Discard the saturated KC1 solution from the tube and clean out the mercurous
-5Q-
TOWOLDMON0028645 WATER_PCB-00013114
chloride and mercury from the Internal element. Clean
parts thoroughly. Add sufficient new clean mercury to the internal element to make contact with electrode wire
and repack chamber of Internal element with mercurous sulfate moistened with 0.5M potassium sulfate. Seal the chamber with non-absorbant cotton. Pill the salt bridge tube with 0.5M potassium sulfate and reassemble units.
9. Burette. 1.0 ml. microburette - Koch - Fisher Scientific Co. - 2C-110.
10. Magnetic Stirrer and glass covered stirring bar.
11. Glass Apparatus for Samples in Bath. See attached diagram.
12. Capillaries. Glass capillaries approximately 0.2 mm in diameter and cut to a length that permits a flow of 45 ml.
per min. of air.
13. Varlac. 2 KVA.
14. Air Supply. Air under 40 lb. pressure is available in our laboratories. This air is purified by passing through a
scrubber bottle containing 40# NaOH, an empty bottle which serves as a safety, a second bottle containing cono. H2SO4 and a trap Immersed in dry ice and acetone. The purified air is connected to a glass manifold having one connection for each sample. Capillaries of the appropriate length are connected between the manifold and the outlet for each sample. In this manner a constant flow of air can be obtained on all samples by applying a constant pressure to
the manifold.
15. Heating Bath, A stainless steel bath constructed according to the specifications given in the attached diagram is used. The bath is heated by applying 85 Volts to 3-5OO Watt G.E. strip heaters bolted to the bottom of the bath. One 500 Watt Immersion heater is connected to the thermostat. Dow
Corning 550 Bilicone is used aB the bath liquid. The tem perature is maintained at 210 + 0,2C. The bath should be placed in hood and the tests carried out in total dark
ness. Two 3 X 5" stainless steel plateB not shown in the sketch are placed on top of the straightening vanes in the bottom of the bath. This provides better stirring to the ends of the bath. Twelve samples can be run in the bath at one time.
Procedure
0263192
Weigh a 290 + 1 g. sample of Aroclor into the 300 ml. Erlenmeyer flask. Insert the gas inlet tube and position the flask in the 210 + 0.5C. bath. The bath fluid level should be approximately one inch below the bottom of the ground glass Joint on the flask. Place 10 ml. distilled water in the Volhard flask absorber and attach to the receiver tube from the Erlenmeyer flask. Connect the purified air supply from the capillary to the Inlet down tube
TOWOLDMON0028646 WATER_PCB-00013115
in the flask. Bubble air through the sample for 16 hours at the rate of 35 to 45 ml. per minute. (The apparatus and/or sample must be kept in the dark during the 16 hour period). Transfer the water from the absorber to a 100 ml. beaker using approximately 50 ml. acetone, and S drops 1$ HNO3 solution and titrate with 0.005N AgNO? solution using a magnetic stirrer. The titration is stopped at 75 mv. which represents the point of maximum potential change and the titration endpoint. Silver wire and mercurous sulfate electrodes (Ag-Hg, HgpSOij, 0.5M K2S04 system) are used for the titration.
Calculations
(Total ml. 0.005 NAgNOj used) (0.6l) > ppm chloride
1 ml. 0.005 NAgNO-a is equivalent to 0.0001773b. chloride or 0.6l ppm.
Precision and Reliability
The precision of the test (standard deviation) is 0.02 ppm at the 0.5 ppm chloride level and 0.06 ppm at the 2.8 ppm lev61. The method as written does not necessarily quantitatively measure the total unstable chlorides present. For screening purposes a total chloride figure is not necessary. Experience has shown that there is good correlation between the chloride figures obtained by this 16 hour thermal stability test and the quality of chlorinated biphenyls.
Discussion
The air supply can be checked for chloride contamination by passing the air through an empty sample flask immersed in the bath. Not more than 0.03 ml. 0.005 NAgNOo should be required to give the endpoint. The air supply oan be checked for ammonia by measuring the pH of the abBorber solution or titrating with 0.01N HC1. The pH should be between 6 and 7. Compressed cylinder air available for breathing purposes can perhaps be used without any purification. Experience has shown that nitrogen gives low chloride figures. This Indicates that air is a neces sary part of this test and that nitrogen cannot be used as a substitute, dum rubber tubing is used in making all connections. The apparatus is cleaned with acetone.
0263193
|
TOWOLDMON0028647 WATER_PCB-00013116
CHAPTER 7 TYPICAL PROPERTIES
The 1200 series members of the Aroclor family are chlor inated biphenyls, and are made by chlorinating biphenyl to approximately the percentage of chlorine, by weight, in dicated by the last two digits of the serial number. For
example, Aroclor 1254 Is approximately 54j6 chlorine on a
weight basis. Accordingly, these Aroclors are not single or simple compounds. They are a mixture of lsomerle com
pounds composed predominately of the chemical compound in
dicated below as being their approximate equivalent:
Aroclor 1242
Trichlorobiphenyl
Aroolor 1S48----------------Totraohloroblphonyi--
Aroclor 1254
Pentachloroblphenyl
Aroclor X2&Q----------------Hcxachloroblphe
flrotlor 1016
1>ichlerc^7pV *
For transformer use and some capacitor U3e
A min\mrvi <
viscosity is required for better low temperature operation
than offered by the above Aroclors, these products are mixed
with pour point depressants, particularly trichlorobenzene
resulting in various denaral Elootrio Company Pyranols 19 nn n 1 3
Trarta former Pyranol 1467*------- 60$ of Aroclor 1260-- *tf># of Eloo. Grade----- *
Trlohlorebenzene 0-. 125^ of Tin Tetraphenyi--
Transformer Pyranol 1470"'
%5% of Aruclur lGo------" 55$ of Eloo. Orade-Trlchloro-*-<-
Te-traehlorobenBono MlJtturc-- 9rl35$t> of Tin Tetraphenylr-*-
relraphehyl scavenger is subject to-
and license: Royalty arrangements should be checked before
using Pyranol 1467. Questions about license concerning the use/*
anthraqulnone stabilizer for DC capacitors should be rgierTed
to We'gtepa-Electrlc. 195 Broadway. N .V, h .
-
0263194
|
TOWOLDMON0028648
WATER_PCB-00013117
TOWOLDMON0028649 WATER_PCB-00013118
I Kier ^ e r\ 10/30
no7o tA dst-rrdhr 3o7o J Z)Luir^JJ (^T-v^&K,
O'ZOTi O'lyC' iJyl 9h<ny) Ziher
A- )3 B38-3
60To d <&* JUwlyr /VjrV yo% oy tM*ij+***P (jrro-Jics
0-lS/o ^ d'HOX 2p*&JUs
0. HOTo oj
2
&-r<- *-t<
ozt-3146
|
TOWOLDMON0028650 WATER_PCB-00013119
AROCLOR 1232
Vlsc.N 37.8C. (ASTM d88)
Specif^ Gravity @ 25/15.5C.
D287)
Color, A I"
Conditic
Clear
Acidity,
.KOH/g.
Pour Point, <\ (ASTM D97)
Inorganic Chlorides, ppm.
Refractive Index^ig 25C.
Distillation Rang\ (ASTM D20)
Corrected for s\pm and
barometlc pressu:
Corrosion
Water Content, ppm Resistivity 100C., 500 volts
DC @ 0.1"gap Dielectric constant 100C.
@ 1000 cycles (ASTM D924)
Sulfates (ASTM-D117-31)* Fixed Chlorine content (Carius)* Dielectric Strength (KV)
(ASTM D877)* Hydrolysis Stability Test
Chlorides, ppm. Thermal Stability Test
Chlorides, ppm.
TYPICAL
44 - 51
1.270 - 1.280 50 Max.
0.014 Max. -30 or lower 0.10 max. 1.6200 - 1.6220
10% - 293C. min. 5056 - 310 - 320 C. 90% - 360C. max. After heating with
aluminum for six hours
at 210C. 10C. the aluminum must not be corroded
either on visual or weight
Inspection and the Aroclor 1242 should meet the following
specB:
Color, APHA
100 max.
Acidity, mg.KOH/g. 0.014 max.
^Inorg. Chlorides,
0.10 max.
CViditlon
dear
35'
500 xVLO Ohm-cm., min. 4.3 - \.5
None
31.5 - 32 .'i 35 min.
3.0 (tentative\max, 0.5 (tentative) max.
*Not determined unless by special request
-64-
0261197
TOWOLDMON0028651 WATER_PCB-00013120
AROCLOR 1242
PROPERTY
---------------------- -- jj
Vise. at^7.8C. (ASTM D88)
Specific Gravity at 25/l5.5C. (ASTM D287)
Color, APHA Condition Acidity, mg. KOH/g. Pour Pt., C. (ASTM D97) Inorganic Chlorides, ppm. Refractive Index at 25 C. Distillation Range (ASTM D20)
Corrected for stem and barometric pressure Corrosion
TYPICAL
82 - 92 seconds Saybolt Univer. 1.381 - 1.392
50 max. Clear 0.01 max. -14 or lower No detectable amount 1.6240 - 1.6260 10?6 325C. min. 90g 360ifl<J..max.
After heating with aluminum for six hours at 210C + 10C, the aluminum must not be cor roded either on visual or weight inspection and the Aroclor 1242 should meet the following specss
Water Content, ppm Resistivity 100C. 500 volts
DC at 0.1" gap Dielectric Constant 100C.
at 1000 cycles (ASTM D924) Flash Point Cleve. Open Cup* Fire Point C.
Sulfates (ASTM-D117-31)* Fixed chlorine content (Carlus)* Specific Heat at 25C.* Evaporation at 100C for 6 hrs.* Dielectric Strength (KV)
(ASTM D877)*
Color, APHA
60 max.
Acidity, mg.KOH/g. 0.01 max.
Inorg.Chlorldes.ppm no detectable
amount
Condition
Clear
35 max.
00 x 109 ohm-cm., min. .7 - 4.9
170 - 200C. None to boiling point None '
403.2$+ 0.5g0
0.4g max. 35 Min.
*Not determined unless by special request.
Hydrolysis Stability Test chlorides, ppm
Thermal Stability Test
chlorides, ppm
1.0 (tentative) max. 0.40 (tentative) max.
-65-
026319
|
TOWOLDMON0028652 WATER_PCB-00013121
AROCLOR 1248
TYPICAL
Vise . \b 54.4C. (ASTM D-88) Spec. Gravity at 65/15.5C.
(ASTM 1\287) Color, AP) Condition
Acidity, mg.xKOH/g. Pour Point C.\(ASTM D-97) Refrac. Index at 20C. Dist. Range (ASTM-.D-20)
\
Water Content, ppm. \
Resist. 100C. 500 v DvC.
at 0.1" gap
\
Dielectric constant, 100%!.
1000 cycle
\
Dielectric Strength 25C.* \
Plash point, (C.O.C.)*
\,
Fixed Chlorine (Carius)*
'
Specific heat at 25C.*
Inorganic chlorides, ppm.
73 80, Sec. Saybold Universal 1.405 - 1.415
100 Max. Clear 0.01 max. -7 1.6285 - I.6305 First drop 310C. min. 10# - 345C. Min. 90g - 385C. Max. 35
500 x 10s Ohm-cm., min.
4.6 35 KV min. 193C. 47.5 - 48.5g \ 0.27 \ 0.10 max.
'Not determined unless by special request.
Hydrolysis Stability Test chlorides, ppm.
Thermal Stability Test chlorides, ppm.
3.0 (tentative)'`max. 0.5 (tentative) max.
-66-
02631"^
|
TOWOLDMON0028653 WATER_PCB-00013122
AROCLOR 1254
PROPERTY
TYPICAL
,
Vise, at 98.9C. (ASTM D88) Specific Gravity at 65/15.5*0.
(ASTM D287) Color, APHA
Condition
Acidity, mg.KOH/g. Pour Pt. *C. (ASTM D97) Inorganic Chlorides, ppm.
Refractive Index at 25"C. Distillation Range (ASTM D20)
Corrected for stem and Barometric Pressure Corrosion
44 - 48 sec. Saybolt Univer.
1.495 - 1.505
100 max. Clear 0.01 max. 7-12 Ho detectable amount 1.6370 - 1.6390 10$( 366 - 378"C.
50# 371 - 383'C. 90# 379 - 394C. After heating with aluminum for 6 hours at 210"C. plus or minus 10"C. the aluminum must not be corroded either on visual or weight inspection and the Aroclor 1254 should meet the following specB:
Water Content, ppm. Resistivity 100"C., 500 v D.C.
at 0.1" gap Dielectric Constant, 100*C.
1000 cycles Dielectric Strength, 25C.* Burn Point (ASTM D92) Sulfates (ASTM D-117-31)* Fixed Chlorine Content (Carlus)* Evaporation at 100C. for 6 hrs.* Stability*
Ageing Characteristics*
Specific Heat at 25C.*
Color, APHA
150 max.
Aoldlty, mg.KOH/g.
0.01 max.
Free Chlorides,ppm.
No detec
table amount
Condition
Clear
35 max.
500 x 10^ ohm-cm., min.
4.15 - 4.35 35 KV, min. Higher than 350*C. None
55 + 0.5* 0.4j^ max.
There shall be no liberation of chlorine or chlorides when the
material is heated at 100'C. in glass vessels in contact with air for periods of at least one month.
No loss in resistivity over original value on heating in air for 96 hrs. at 100C. 0.26
*Not determined unless by special request.
Hydrolysis Stability Test Chlorides, ppm.
Thermal Stability Test
Chlorides, ppm.
3-0 (tentative)max. 0.5 (tentative)max.
0263200
TOWOLDMON0028654 WATER_PCB-00013123
AROCLOR 1260
PROPERTY
v\o. at 98.9c. (ASTM d88)
Specific Gravity at 90C./15.5C. ;a\tm D287)
Color\APHA Condition A c i d i t y\mg. KOH/g. Pour Pt.XC.(ASTM D97) InorganicVhlorides, ppm. Refractive \ndex, 25C. DistillatiorrvRange (ASTM D20)
Corrected s\r stem and barometric pressure. Corrosion
TYPICAL
72 - 78 Sec. Saybolt Unlv. 1.555 - 1.566
150 max. Clear 0.01 max. 25 - 34 No detectable amount 1.6455 - 1.6470 10# 385 - 398C. 50^ 390 - 4o4C. 90$ 400 - 420C. After heating with aluminum for 6 hrs. at 210C. + 10C. the aluminum must not be cor roded either on visual or weight inspection and the Aroclor 1260 should meet the following specs;
Water content, ppm.
.
Resistivity,100C. 500 volts
at 0.1" gap
Dielectric Strength 50C.*
Dielectric Strength 100C.*
Dielectric Constant 100C.
at 1000 cycles*
Burn Pt. (ASTM D92)*
Sulfates (ASTM D117-31)
Fixed chlorine content (Carius)*
Evaporation at 100C. for 6 hrs.*
Stability*
Specific Heat at 25C.*
Color, APHA
150 max.
Free Chiorides,ppm. No detec
table amount.
Acidity,mg.KOH/g. 0.01 max.
Condition
Clear
35 max,
500 x lO^ ohm- cm., min.
30 KV., min. 30 KV., min.
,6 - 3.8
Higher than 350C.
NoneS 60 + 0.2$ ma
There slifcUl be no liberation of chlorine or chlorides when
the material is heated at 100C. in a glass vessel in contact with air for periods of at least one month.
0.23
*Not determined unless by special request.
Hydrolysis Stability Test chlorides,ppm.
Thermal Stability Test chlorides, ppm.
3.0 (tentative) max. 0.7 (tentative) max.
-68-
0263201
I
TOWOLDMON0028655 WATER_PCB-00013124
PYRANOL 1481
Viscosity 'Swt 3T.8C. Spec. Gravity at 15.5/15.5C. Color, APHA Condition Acidity, mg. KOH/ Pour Pt., C. Inorganic Chlorides ,\ppm. Refractive Index at 25^C. Distillation Range
Corrected for stem and
barometric pressure. First drop
25$ max. 90$ Corrosion Test Change in Weight Color, APHA Acidity, after test, mg.KOH/g. Free Chlorides, ppm.
Condition after test Water Content, ppm.
Resistivity at 100C 500 volts, DC, 0.1"gap
Dielectric Constant (100C., 1000 cycles)
Hydrolysis Stability Test chlorides, ppm. .
Thermal Stability Test chlorides, ppm.
TYPICAL
70 - 82 sec. Saybolt Unlv. 1.525 - 1.535 150 max. Clear 0.01 max. -15 or lower 0.10 max. 1.6205 - 1.6215
205C. min. Below 270C. 380 - 395C.
0.0$
200 max. 0.01 max.
.10 max.
lear 35Vax.
100 X\lo9 ohm-cm.,min.
4.1 - 4\6
3.0 (tentative) max.
0.5 (tentatiVe) max.
-69-
0263202
TOWOLDMON0028656 WATER_PCB-00013125
PYRANOL 1488
OPERTIES
Vi\. at 37.8C.
Spec\ Grav. at 15.5/15.5C.
Color \APHA
AcldityMMg KOH/g)
Water, ppm.
Condition \
Refrac. InaXx at 25C.
Free Chloridd, ppm.
Pour Point, C\
Reals, at 100C\ 500 v D.C.
1" gap
\
Dielectric Strength (25C.)
Corrosion:
\
Loss of Aluminum \
TYPICAL
54-2 Sec. Saybolt Univ.
1.560 - 1.568
150 max.
.014 max.
35 max. Clear
1.6137 - 1.6147
0.10 max.
'
Lower than -32C.
100 x 109 ohm-cm min. Over 35 KV
None Heating with aluminum for 6 hrs. at 200-220C. The Pyranol after heating should meet the following specs:
Dielectric Constant at 1000 cycles at 100C.*
Listllling Range (corrected)* 1st drop Below 270C. 90$ point
Burn Point (ASTM D-92)* Fixed Chlorines*
Arc Formed Gases*
(Oxygen-free liquid at 25C.)
Color, APHA
Acidity (MgKOH/g) Free Chlorides ppm
Condition
200 max. .014 max .10 max.
Clear
- 4.0
200\. min. 4o$ max.
295 - 415C. None up to boiling point
59*1$ min. Less than 1 .'8$ total com bustible gases\includlng
carbon monoxlde\hydrogen, and volatile hydrocarbons.
*Not determined unless by special request.
0263203
|
TOWOLDMON0028657 WATER_PCB-00013126
PYRANOL 1467
1 OPERTIES
TYPICAL
VisJs. 37.8C., (ASTM D88)
Srec? Gravity at 15-5/l5-5C.
I M D-287)
Colot PHA
Conditio:
Acidity, ir()j
g,
Pour Point,
ASTM D-97)
Inorganic C
es, ppm.
Refractive
at 25C.
Dlstillatic
e (ASTM D20)
Corret
r stem and
barome
measure
Corrosion
54+2 sec. Saybolt Univ.
I.560 - I.568 150 max. Clear 0.01 max. -32C. or lower 0.10 max. 1.6137 - 1.6147 1st drop - 200"C. min. Below 270"C. - 40J6 max. 90?! - 395 - 415"C. After heating with aluminum for 6 hrs. at 200-220"C., the aluminum must not be corroded either on visual or weight in spection and the Pyranol should meet the following specs:
Color, APHA Acidity, mg.KOH/g. Inorganic Chlorides
ppm. Condition
200 max. 0.01 max. 5 itiax.
Clear
Water Content, ppm. Resistivity, 100"C. 500 volts,
0.1" gap Dielectric Strength, 25C. Dielectric Constant, 100"C.
1000 cycles* Tin Tetraphenyl*
Burn Point, (ASTM D92)*
Fixed Chlorine* Arc Formed Oases*
(Oxygen Free Liquid at 25C.
30 max.
Q 100 x 10' ohm-cm. 5 KV., min.
min.
3>7 - 4.0 O.IC556 + 0.01$ by weight Nonevup to Boiling Point
59.15&Vin. I.O56 ustible gases carbon monoxide,
a^d volatile hydro-
*Not determined unless by special request -71-
026320"'
TOWOLDMON0028658 WATER_PCB-00013127
PYRANOL 1470
TYPICAL
at 37.8C. (ASTM d88) Spec.\Gravity a4t- T1C5-5c//n1c5. 5C C.,
(ASTM\D287) Color, aSPHA
Conditions
Acidity,
KOH/g.
Pour Pt., C\, (ASTM D97)
Inorganic Chlopldes, ppm.
Refractive Inddx at 25C.
Distillation Range (ASTM D20)
Corrected for stdm and
barometric pressur First drop
35/ 55/
65/
95/ Corrosion
41-45 Sec. Saybolt Univ.
1.563 - 1.571 150 max. Clear' 0.01 max. -44C., or lower 0.10 max. 1.6075 - I.6085
., min. 256C. 330C. 400C. . 4l5c. After heating with aluminum for 6 hrs. at 200-220C., the aluminum must not be corroded either on visual or weight inspection and the Pyranol should meet the following specs:
Water Content, ppm. Resistivity, 100C., 500 v.,
0.1"gap Dielectric Strength, 25C. Dielectric Constant, 100C.,
1000 cycles* Tin Tetraphenyl* Burn Point, (ASTM D92)* Fixed Chlorine* Arc Formed Oases*
(Oxygen Free Liquid at 25C.)
Electrical Stability*
Color, APHA
200 max.
^Acidity, mg.KOH/g. 0.01 max.
aorg.Chlorides,ppm 5 max.
C6nditlon
Clear
30 m^x.
100 x
ohm-om., min.
35 fcV.,>in.
3.8 - 4.3>'
0.125/ + 0.\l/ by weight None up to Bolling Point
60.5 + 0.5 Total combustible gases in cluding carbon nionoxide, hydro gen and volatileNhydrocarbons.
After heating for\?6 hrs. at 100C. in a closed\container, the resistivity should not
decrease more than lC `
*iJot determined unless by special request.
-72-
0263205
|
TOWOLDMON0028659 WATER_PCB-00013128
INERTEEN PPO
Visc\@ 37.8C. , (ASTM D88) Specific Gravity @ 15.5/15.5
(ASTM D-287) Color AP'SA Condition! Acidity, mg.. KOH/g. Pour point, \C. (ASTM D-97) Inorganic Chlorides, ppm. Refractive Index @ 25C. Distillation ra\ge (ASTM D20)
Corrected fqr stem and barometic pressure Corrosion
Water content, ppm. Resist., 100C. 500 Volts,
0.1" gap Dielectric Strength, 25C. Dielectric constant, 100C.
1000 cycles* Phenoxy Propene Oxide or Glycldyl Phenyl Ether Burn point, (ASTM D92)* Fixed Chlorine* Arc formed gases* (Oxygen free liquid @ 25C.
TYPICAL 54^ 2 sec. Saybolt Universal
I.56O - 1.568 150 max.
Clear 0.014 max.
-32C. or lower 0.10 max.
1.6137 - 1.6147 First drop - 200C. min. Below 270C. - 40# max.
90# - 395 - 4l5C. After heating with aluminum for 6 hours at 200 - 22CC. the aluminum must not be corroded either on visual or weight inspection and the askarel should meet the follow
ing specs:
Color, APHA
200 max
Acidity, mg.KOH/g.
0.014 m
Inorganic Chlorides, ppm. 2 max.
Condition
Clear
30 max.
100 x 10 Ohm-cm., min. KV., min.
4.0 - 0.22# by weight
None 'Jw to boiling point
59.1# min. Less than 1.0# Total combustible gases includingVarbon monoxide, hydrogen anq volatile hydro
carbons .
*Not determined unless by special request.
02|
TOWOLDMON0028660 WATER_PCB-00013129
CHAPTER 8
QUALITY REQUIREMENTS OF ARCCLORS PRIOR TO USE IN THE ELECTRICAL INDUSTRY
Quality aa Supplied to the Electrical Industry Aroclors and their mixtures supplied to the electrical
industry must meet the strict requirements specified by the industry and given in the specifications shown in Chapter 7 The electrical qualities, such as resistivity and power factor of the materials, as supplied, are not the maximum attainable. It is impractical for the manufacturer to furnish these dielectrics to the customer at the maximum attainable qualities because even with careful packaging, sampling, shipping, and handling, these fluids may pick up traces of contaminants from "clean" tank cars, drums, pipe lines, pumps, etc. However, as supplied in accordance with the specifications, the fluids must respond readily to "up-grading" by earth treatment to arrive at the desired maximum refinement required for use by the electrical Industry.
Typical Electrical Quality of Aroclors Used in the Industry-
Capacitor Impregnation
Table IV indicates the desirable minimum resistivity
values of Aroclor dielectrics immediately after earth refinement
by the user when ready to impregnate capacitors. These values
arc compared with the similar values of the material after the
capacitor impregnation has been completed in a relatively clean
system.
0263207
TOWOLDMON0028661 WATER_PCB-00013130
TABLE IV
Dielectric
Volume Resistivity Ohm-cm at
100C. and 500 volts DC.
Prior to
After
impregnation
Impregnation
Aroclor 1254
2.500 x 108
890 x 109
Aroclor 1242
1.500 x 10s
600 x 10 s
-Pyranol 1481
eoo-x-ie^-
4ee
The power factor of earth refined Aroclor prior to capacitor
Impregnation should not exceed 0.1 percent at 100C. and 1000
cycles.
Transformer Pilling The minimum resistivity of transformer askarel as specified for supply to the electrical industry Is 100 x 10e Ohm-cm. at 100C., 500 volts and 0.1 inch gap. While power factor is not part of the suppliers' official specification, this value for freshly made transformer askarel ranges from 0.1 to 0.3 percent at 100C. and 1000 cycles. This would be approximately 0.05 percent at 20C. and 60 cycles. In order to arrive at higher and yet practical dielectric valueB the transformer manufacturer needs to earth refine the fluids immediately prior to using. It Is reasonable to strive for a volume resistivity value around 1,500 x 10s Ohm-cm. at 100C. and power factor values of about 0.05 percent at 20C. and 60 cycles or 2 percent at 100C. and 60 cycles.
-75-
026 32 00
TOWOLDMON0028662 WATER_PCB-00013131
Table V compares resistivity readings with the corres
ponding power factor values obtained on the given samples of
typical transformer askarel.
TABLE V
Volume ReslBtivlty 10B Ohm-cm. at 10QC.
Power Factor 60 cy. 1Q0C. 60 cy. 20C.
1,500
256 0.05$
500 100 60-70
556 1556 ' 20-2556
O.156 0.756 2.056
When adequately earth refined to give a resistivity in
the range of 500 to 1500 x 10s Ohm-cm. at 100C., sample of
such transformer aBkarel taken after filling a newly constructed
and relatively clean transformer should have a resistivity of at
least 200 x 108 Ohm-cm. at 100C. and a corresponding power
factor less than 12 percent at 100C. and 60 cycles.
-76-
02b320q
TOWOLDMON0028663 WATER_PCB-00013132
CHAPTER 9
EARTH REFINEMENT OF AROCLORS TO ARRIVE AT THE DESIRED ELECTRICAL QUALITIES
Earth Treatment In the Laboratory Preparatory to Analysis In Chapter 5 on Page 27 the laboratory procedure
for preparing the test sample using 0.1 to 0.2 percent of activated earth is given. It is also stated that the absorbent is minus 200 mesh Attapulgus earth activated Just prior to use by heating in shallow trays for four hours at 400C. (752F.) or for at least 12 hours at 250C. (482F.)
Earth Treatment by the Plant Manufacturing the ABkarel
Earth refinement in the plant is essentially the 3ame
as used when preparing the laboratory sample. The same amount .wP +0
of freshly conditioned earth (T).l percent to 0.2 percent by
weight) is added to the askarel and the mixture is agitated
thoroughly and heated for about four hours.
The more viscous dielectrics, such as Arroolor 1C|I,&--^--
gan^ Aroclor 1254> are heated at about 70 to 8oC. (158 to 176P.),
^ and-lhe les3 viscous materials such a3 Aroclor 1242 and Pyranals--*
-3-----l4Sir;--1467 and-1470, -or Inarteon PPO are heated at about 50
to 60C. (122 to 140P.)
0263210
After about four hours contact the earth is removed
from the dielectric fluids using a Sparkler or Sweetland or a
comparable filter press, previously fitted with filter paper jpnrkicr Filft r CatforMtiot, Conrad,
liners such as supplied by Carl Schle lidim1 & Schuel-ecmipany
7?yc
Kanno, Mow Hampshire The paper is
-77-
TOWOLDMON0028664 WATER_PCB-00013133
and must be dried at 100C. to remove moisture prior to use in the filter press. Earth Refinement by the User
Capacitor Manufacturers: Capacitor manufacturers usually use the same procedure for earth refining as employed by the manufacturer of the askarels. Because this method employs loose earth which can be thoroughly mixed Into the askarel, it is believed to be the most efficient and Is certainly known to give very good results. However, towers (cylinders) filled with relatively coarse earth through which the dielectric fluids are pumped and recirculated have also been used by capacitor manufacturers.
Transformer Manufacturers; The large manufacturers of askarel transformers usually use the same type of procedure for refinement with loose earth as employed by the manufacturer of the askarel dielectrics. Handling relatively large amounts of the askarel transformer fluid Justifies Installing the tanks and filter presses required. This earth refining equipment is usually supplemented with portable cartridge type filters or a small portable platen frame type filter press. This latter equipment is then used when newly made askarel transformers are filled with the fluid and it is necessary to clean the transformer and the fluid by draining out the fluid pumping it through the filter press or cartridges containing the earth and recirculating until the desired electrical properties are attained.
Likewise, smaller manufacturers of askarel transformers can use most conveniently the portable cartridge or platen frame
typf' fllters.
-78-
<,*63211
TOWOLDMON0028665 WATER_PCB-00013134
The Effect of Earth Refinement on Removal of
--
--Tetra phenyl Scavengers from the Transformer Askarel: As Indicated
above, normally transformer askarels respond readily to up-grading
by the use of 0.1 to 0.2 percent by weight of earth based on the
total weight of the fluid. However, If the fluids are unusually
contaminated, larger amounts of earth are required to up-grade
the dielectrics. This raises question about the selective
adsorption of the scavengers by the earth treatment. It 1b
Indicated that to selectively adsorb significant amounts of the
scavengers, repeated treatment with 1 percent or more of earth
is required, as shown In the following tablei-'*--
REMCfflAL-OF TIN--TETRAPHEHYL BY, REPEATED TREATMENT --OF-A&KAftEL WITH TIKE PERCENf-QP EARTH------ q?
-79-
0263212
TOWOLDMON0028666 WATER_PCB-00013135
CHAPTER 10
CONTAMINATION Askarels as supplied by the manufacturer respond readily to earth refining resulting in a very high order of dielectric properties. For example, it is possible to attain volume resistivity values up to 20,000 or 30,000 x 10^ Ohm-Cm. at 100C., 500 volts, 0.1 inch gap and power factor values no more than 0.05# at 100C. and 1000 cycles. Except for very special situations, it is not practical to refine these dielectrics to this extent. In commercial use, transfer of the fluids from one clean container to another which may result in contacting traces of conducting impurities does not allow maintaining such a high order of dielectric properties. Referring to electrical values, this accounts for the more practical order of specification values as indicated in Chapter 7 and to which the electric Industry has committed the supplier of the dielectrics. This also accounts for the desirability and need of the user of askarel dielectrics to earth refine Immediately prior to use in order to arrive at the maximum and yet practical dielectric values for his given purpose. Such quality values relative to askarels for capacitors and transformer work were indicated in the preceding Chapter 8.
AVOIDANCE OF CONTAMINATING ASKAREL CAPACITORS It is necessary, practical and economical that all steps possible be taken to avoid contaminating influences in the manu facture of askarel capacitors.
-80-
0263213
TOWOLDMON0028667 WATER_PCB-00013136
Sometimes capacitor manufacturers strive to attain the very
high order of dielectric qualities possible for askarel as mentioned
above. Since it is very difficult, if not almost impossible to
maintain such a high order, usually capacitor manufacturers comply
with the more practical schedule attainable by normal earth
refining practices as shown in Table IV Chapter 8.
Equal care must be exercised in selecting, conditioning and
handling the other construction materials of the askarel capacitor.
For example, the water used in manufacturing capacitor tissue is
either distilled or deionized. Quality control of the capacitor
paper requires chemical tests to characterize the fiber and its
purity. Physical and electrical tests to determine moisture and
power factor are essential. Acceptable dielectric loss values of
the dry and unimpregnated paper do not suffice for Judging quality
because in some Instances after impregnation with good quality
askarel, higher dielectric losses Increasing rapidly with temperature
may be obtained.
The aluminum foil used must be extremely pure and free from
residual traces of rolling oils or compounds. Accordingly, the
term usually applied to the foil is "dry" foil. Similar care and
purity requirements apply to the aluminum tabs used.
The paper and aluminum foil is wound to form the core in an
air conditioned room and often the machine operators are required
to wear cotton gloves to prevent oil from the operators skin
contaminating the cores.
0263214
The steel cans or turn plate capacitor cans require thorough
cleansing and degreasing with perchloroethylene of required purity
and free of any objectionable stabilizing agents. -81-
Similarly, the
TOWOLDMON0028668 WATER_PCB-00013137
capacitor Impregnating equipment and chambers must be kept clean.
To facilitate maintenance of cleanliness, sometimes stainless
steel construction is used. However, ordinary steel equipment
Is common and when "conditioned1', that Is to say, coated with a
thin film of clean Aroclor, this type of construction material is
entirely satisfactory. To condition a new plant or clean an old
one, askarel is circulated through the system, then purified by
earth refining and recirculated. This process is repeated until
all contaminating influences have been removed.
Moisture, probably the most obvious contaminent In askarel
impregnated capacitors. Increases the dielectric loss under AC .
voltage and decreases the capacitor life. Therefore, very efficient
vacuum, as low as 5 or 10 microns, and heat carefully controlled
up to 130C. are employed to expel the moisture from the capacitor
cores prior to Impregnation. Also to avoid moisture entering the
askarel during storage. It Is common practice to warm the dielectric
In the storage tank to about 50C. In the presence of mild vacuum.
Traces of any substances soluble in askarel and capable of
ionization will have a marked adversed effect on the dielectric loss of the askarel or the finished capacitor. Therefore, much
r
care is required to avoid contamination with solder flux. For
example, the use of rosin core solder is known to cause contamination.
When rim sealing compounds are used in the lids of small capacitors,
there must be assurance that the catalyst or other ingredients
used in such materials do not cause contamination. Improperly
selected pipe sealing compounds used on the threads on the fittings
for sight glasses and Instruments on the storage and impregnating
equipment are known to have caused contamination. -82-
026321^ TOWOLDMON0028669
WATER_PCB-00013138
**+****
All these factors about contamination must be kept in mind when impregnating capacitors, especially by the chamber method but also by the manifold method.
The moisture content of the paper used in the capacitor cores may easily introduce several gallons of water into the average Impregnating chamber. This water is removed from the capacitors prior to impregnation -- usually by heating the chamber to 130C. in the presence of efficient vacuum, 100 microns or less.
If the chamber is not made of the preferred materials of construction, slight corrosion (Iron rusting) may occur and the film of askarel on the interior surface of the tank may become contaminated and introduce traces of impurities into the clean dielectric fluid entering the chamber for impregnating the capacitors. In fact, because of this possibility of contamination, in some operations the capacitors are conditioned and dried in a separate oven or chamber. Then when thoroughly dried, they are then transferred into a second chamber used only for impregnation.
In the case of relatively large sized capacitors, such as power factor correction units, a manifold with branches may be used to handle each unit individually rather than by the batch -- chamber method.
The unimpregnated capacitors are placed into an oven and vacuum is applied to the individual units attached to the manifold. After the capacitors have been evacuated and dried, the askarel is introduced through the manifold and its branches. Care must be taken that moist air or contaminants do not collect in the branches through which the dielectric is introduced.
***#**
-82A-
0263216
|
TOWOLDMON0028670 WATER_PCB-00013139
Care must be taken to avoid contamination with any kind of grease, oil, packing material and "rubber" gaskets used with the machinery, such as pumps, etc., connected with the handling and Impregnating facilities.
It Is not practical to discuss all possible sources of contamination and it should suffice to say that the manufacturers of askarel capacitors need to and do exercise all known precautions to avoid contamination and should evaluate and life test represent ative units before supplying the finished merchandise.
AVOIDANCE OF CONTAMINATING ASKAREL TRANSFORMERS Obviously, in the manufacture of askarel transformers it is
Impractical and impossible to employ purification or refinements
as required, for example, in the production of askarel power factor
correction capacitors.
In a transformer, heat from the dielectric losses of "slightly"
contaminated askarel is negligible compared with heat generated
by the transformer core. While power factor and resistivity of the
transformer fluid are important, they are not as critical as is
the case when similar askarels are used in capacitors.
However, this does not excuse the aBkarel transformer manufac
turer from striving to meet the practical quality requirements as
given In Chapter 8. In order to meet these requirements, it is
necessary to earth refine the transformer askarel immediately prior
to filling the unit. After the initial fill, the fluid should be
withdrawn from the transformer, circulated through an earthen filter,
then pumped back into the transformer and recirculated through the
filter until both the fluid and transformer are clean and show the
desired power factor and resistivity values. -83-
02*>3217
TOWOLDMON0028671 WATER_PCB-00013140
If such normal earth refinement fails to give the desired
results, it will be necessary to study the quality of the materials
of construction and look for all possible sources of contamination
in the transformer and handling equipment.
The characteristic high dielectric strength of transformer
askarel is not a good criterion of purity because with the exception
of being adversely affected by moisture, it is not impaired irre
spective of the contamination of soluble products which give increased
power factor. F. M. Clark of General Electric Company tabulated
the following values of transformer askarel selected from hundreds of
askarel samples taken from commercially operating transformers to
show lack of reduction of dielectric strength with marked increase
of power factor values.
TABLE VII
DIELECTRIC STRENGTH AND POWER FACTORS OF ASKAREL IN USED TRANSFORMERS
Sample
Power Factor, 60 oy. at 25C., per cent
Dielectric Strength at 25C. KV
No. 1
0.1 33
No. 2 No. 3 Mo. 4 No. 5
0.5 5 15 30
35 45 39 43
However, the need for care and proper selection of transformer
construction materials is emphasized in the following tabulation
which shows the marked increase of power factor resulting from
contamination of the askarel with synthetic rubber materials and
varnished cloth, as compared with acceptable materials of construction
given in Table VIII.
,,
TOWOLDMON0028672 WATER_PCB-00013141
TABLE VIII
POWER FACTOR CONTAMINATION PRODUCED BY TRANSFORMER MATERIALS AOED IN ASKAREL AT 100C. FOR 96 HOURS
Material
None Black varnished cloth
Askarel Power Factor, Percent
1.0
85.0
Dielectric Strength, KV
35
42
Copper Press Board Manila Paper Phenolic resin
1.52.0
1.5 1.6
40 37 39 4i
Shellac
6.0 36
Iron
5.0 39
Synthetic rubber
70.0
39
Contaminants which cause a high power factor will of course
also impair resistivity values.
The following Table IX Bhows the degree to which acceptable
and good commonly used materials of construction lower resistivity
from the original high values possessed by the askarel.
TABLE IX
EFFECT OF COMMONLY USED INSULATION MATERIALS ON THE RESISTIVITY OF TRANSFORMER ASKAREL
Sample
Volume Resistivity x lQg Ohm-cm. at 100C.
1. Freshly made askarel before heat aging
2,000
2. Same as 1, after heat aging
1,900
3. After heat aging with the following materials added
a - Phenolic resin tap changer material b - paper
c - Grade A press board (tan)
1,200 750
500
0263?19
|
TOWOLDMON0028673
WATER_PCB-00013142
d - Grade A press board (gray) e - Grade A press board, laminated strip f - Cotton wrapping
g - Glyptal 1276 cement, cured 48 hours at 110C.
500 400 300
100
The procedure used to evaluate materials of construction
Is simple and should be employed by all makers of askarel trans
formers.
One Inch square samples of the surface of the construction
materials are immersed In one liter of good quality transformer
askarel and heated for 96 hours at 100C. The increase In power
factor and reduction of resistivity of the fluid after such exposure
are compared with the values of the original fluid heated similarly
but In the absence of the construction materials.
The following Table X gives such a comparison and Illustrates
the unacceptable properties of the varnished cambric and black
binding tape.
TABLE X
PROPERTY
FRESHLY MADE TRANSFORMER
ASKAREL
PF, 100C., 1 KC
Resistivity,Q100C. Ohm-cm. x 10y
0.2$ 2,500
SAME FLUID EXPOSED TO FIBER BOARD VARNISHED CAMBRL
OR BLACK BINDING TAPE
0.45$
3$
436 18
Dielectric Strength at 25C.
45 KV
45 KV
45 KV
When the askarel fluid contaminated with varnished cambric or
the black binding tape was treated for one hour at 75C. with one
percent by weight of attapulgus earth, the power factor and resistivity
values were restored to those of the original fluid.
0263220
|
TOWOLDMON0028674 WATER_PCB-00013143
While there seem to be no reports of askarel transformers
failing in service as a result of contamination from the use of
questionable materials of construction, as discussed above, their
unwise use is readily detectable and leads to embarrassing question
about impairment of the transformer's life.
Such a case is illustrated by an askarel transformer giving
a megger reading reading as low as 3, after two years service life.
The transformer had not been subjected to arcing and the dielectric
strength of the askarel remained above 35 KV at 25C., or well
within the specification of new askarel. Maintenance of high
dielectric strength in the presence of contamination appears to
account for the transformer not falling.
The following Table XI compares the properties of freshly
made askarel with the similar values of the fluid taken from the
transformer after two years use and also with the same contaminated
fluid following refinement by earth treatment.
TABLE XI
COMPARISON OP PROPERTIES OP CONTAMINATED TRANSFORMER ASKAREL BEFORE AND AFTER EARTH REFINEMENT
PROPERTY
TYPICAL OF NEW ASKAREL
SAMPLE FROM TRANSFORMER
USED 2 YEARS
SAME SAMPLE AFTER EARTH TREATMENT 1 HOUR WITH 1$ OF EARTH
PF., 100C. 60 Cycles
1 to 2$
PF., 100C. 1 Kc.
0.2$
Resist. 100C Ohm-cm. x 10 500 to 1500
150$(dissipation factor)
1556
6
1$ 0.1$ 2600
Dielectric Strength 25C
Moisture ppm.
45 25
40 80
45 20
Acidity mg. KOH/g. 0.01
0.02
0.005
Color APHA
TO
1000 -87-
275 0263221
TOWOLDMONOQ28675 WATER_PCB-00013144
In the above case it was determined that a varnished insula
ting material used in the transformer waB the source of contamination
Since this continuously dissolved in the askarel, obviously, removal
of the fluid, followed by earth refinement and refilling the trans
former accomplished nothing. The situation pertained at the time
of the initial fill persisted until the deleterious component was
removed.
Newly built or rebuilt transformers using acceptable materials
of construction often contain undeterminable traces of impurities
and "dirt" which effect power factor and resistivity, but can be
removed by repeated flushing with clean askarel. The following
Table XII compares the properties of the askarel sampled after the
initial fill with similar values after earth refinement and "soaking"
or flushing the transformer, twice with good askarel. After the
"dirt" or contamination was removed from the transformer the askarel
fluid remained in good condition in the unit as Bhown in Table XII.
TABLE XII
PROPERTY
SAMPLE AS RECEIVED
AFTER TREATMENT
Resistivity @ 100C.
30 x 109
2600 x 10
Dielectric constant @ 100C.
3-9
3-9
Power Factor @ 100C., 1000 Cycles 2#
0.27#
Moisture
60 ppm.
25 ppm.
Moisture solubility in askarel at 25C. is about 110 parts
per million and the specification for new askarel allows a maximum
of 30 parts per million of water.
Essentially, moisture-free askarel was found by Clark to have
a dielectric strength of 70 KV. With Increased amounts of dissolved
-88-
0263222
TOWOLDMON0028676 WATER_PCB-00013145
water the dielectric strength gradually decreased and appealed to level off at a value of about 38 KV when the water content reached 80 parts per million.
Water exceeding tne solubility limit in askarel has a marked adverse affect on the power factor and resistivity of the dielectric fluid, which mar, however, maintain its high breakdown strength even though water accumulates as a separate phase on the surface.
Undissolved moisture can be removed readily from transformer askarel by warming the fluid to 70C. and blowing with dry nitrcger or by treatment with dry, conditioned earth and filtering through a press fitted with dry filter papers or through an earthen cartridge type filter.
As indicated previously, moisture must be kept out of askarel transformers by using adequate gaskets, as described in Chapter 3, and preferably sealing the device with dry nitrogen over the askarel.
Mineral oil is soluble in these fire-resistant transformer askarels and is regarded to be a contaminant. Petroleum hydro carbons cannot be removed from askarels and the permlssable amount may not exceed 2 percent by volume lest the fire-resistant values of the askarel is impaired beyond acceptable limits.
Possible contaminants in transformer manufacture include welding and solder fluxes, oils and greases, bituminous materials, pipe thread lubricants, and contamination from bushing and pot head compounds. Paint or varnish coatings must not touch the interior of the transformer shell.. Adhesives or coatings applied to gaskets must not touch the interior of the transformer.
-89-
02b3223
TOWOLDMON0028677 WATER_PCB-00013146
All natural or synthetic rubber plastics or polymeric
materials, resins, varnishes and lacquers and adhesives must be
regarded as contaminants unless included in the very few acceptable
classes and proved suitable by actual testing.
It is disappointing to find an askarel transformer manufacturer
exercising precautions against contamination, and employing earth
refinement, and yet inadvertently using a neoprene or other
objectionable hose line to transfer the fluid economically!!
If flexible hose needs be used, it should be a flexible stainless
steel type or a "rubber" hose lined with Teflon.
When using any of the following suggested suitable materials
of construction, it is prudent to employ appropriate oontrol evalua
tion tests to be certain that the given material within a class
regarded as acceptable will meet the requirements from a physical
and electrical standpoint.
TABLE XIII
ACCEPTABLE MATERIAL FOR CONSTRUCTION OF ASKAREL TRANSFORMERS
Structural Materials and Fillings
Metals - Commonly used metals Including steel, copper, aluminum, tin and brass are suitable if clean.
Wood - Suitable if dry and free of natural gums and resins.
Paper - Suitable
Press Board - Suitable
Cotton - Suitable
Asbestos - Suitable
Glass - Suitable --------Ceramics - Suitable
. 0 Z632?'*
Phenol-formaldehyde resins - Suitable if adequately cured.
-QO-
TOWOLDMON0028678 WATER_PCB-00013147
Melamine-formaldehyde resins - Suitable If adequately cured. Cellulose acetate - Suitable Cellulose tri-acetate - Suitable Cork - Suitable Gasketing Materials and Adhesives Metals - (As above) Teflon - Suitable Silastic (silicone) - Suitable if adequately cured. Polyurethane - Suitable if adequately cured. Cork (fine grain and bonded with phenolic resin) - Suitable,
but susceptible to penetration by askarel. Nitrile rubber - Sometimes used for gaskets - but susceptible
to attack by askarel. Cork Nitrile rubber - Often used Dewaxed Orange Shellac - Suitable Epoxy - Suitable If adequately cured. Isocyanate - Suitable if adequately cured. Tar.es and Wire Insulation Cotton - suitable Paper - Suitable Asbestos - Suitable Glass - Suitable Rayon - Suitable Cellulose acetate - Suitable Teflon - Suitable Silicone - Suitable
-91-
0263225
TOWOLDMON0028679 WATER_PCB-00013148
Surface Coating; for Transformer Exterior Baked Phenol-Formaldehyde - Suitable Baked Melamine-Formaldehyde - Suitable Baked Epoxies - Suitable Polyurethane Coatings - Suitable
Surface Coating for Interior of Transformer Shell to Prevent Rusting in Storage
25 parts Aroclor 5460 dissolved in 75 parts lacquer thinner.
The need for clean shop practice and avoidance of contaminating influences when building askarel transformers is emphasized by the following information submitted by a highly qualified manufacturer to indicate the condition of askarel sampled from normally opera ting apparatus after a number of years service. Fluid sampled from the top and bottom of at least 25 askarel transformers operating satisfactorily in different part of the country was analyzed, comprehensively. The following general conclusions were drawn:
1. The residual condition of the askarel samples for the most part was satisfactory, but in a few Instances excessive dirt or sediment was noted.
2. Moisture content ranged from 19 to 6l parts per million with most samples between 25 and 35 ppm. This reflects a very good degree of dryness.
3. Acidity values were all below 0.01 mg. NaOH/g., which corresponds with the level of freshly made askarel.
"92-
0P63226
TOWOLDMON0028680 WATER_PCB-00013149
4. In most cases the free chlorides did not exceed 0.1 ppm., the specification limit of new askarel. The highest reading was 0.15 ppm.
5. Dielectric strength values ranged from a maximum of 46 KV to a minimum of 28 KV which values are considred satisfactory.
6. Volume resistivity at 100C. ranged from 20 to 75 x 10B Ohm-cm. which is considered to be satisfactory and may be compared with the specification for new askarel at 100 x 10e Ohm-cm., minimum.
7. Power factor values at 100C. and 60 cycles ranged from 19 to 75 percent with most samples below 60 percent.
From the above data considered typical and satisfactory relative
to all of these askarel transformers operating in a normal manner,
it is seen that under satisfactory service life the resistivity of
the askarel will decrease and the power factor will increase, as
Indicated, from similar values of fresh askarel.
These observations emphasize the need for askarel transformer
makers to:
1. Earth refine the askarel immediately prior to use
in order to arrive at the highest practical electrical
values from the fluid.
2. Avoid construction materials which are a source of contamination
3. In using acceptable and satisfactorily tested construction
materials - to flush the transformer to remove traces of
contaminating influences and "dirt". -93-
0263227
TOWOLDMON0028681 WATER_PCB-00013150
CHAPTER 11 REWORKING CONTAMINATED TRANSFORMER ASKAREL Normal Conditions Aakarel contaminated during manufacture of the transformer or after years of normal service life should respond very readily to refinement by treatment with a few tenths of a percent of dry Fullers earth, or Attapulgus clay. This was discussed in detail in previous chapters. About askarel transformers, after years of normal service life and having continued satisfactory performance, question (difficult to answer) arises as to how high may be the power factor. Also, how low may be the volume resistivity. The case histories given in the preceding chapter seem helpful in arriving at an answer. Doble Engineering suggests to their clients that, "When used askarel is found to have a power factor of 2.0 percent or more, the cause of high power factor should be determined." (This refers to power factor measured at 20C. and 60 cycles.) Doble qualifies this suggestion stating, "If the high power factor is caused by water or other conducting matter, free chlorides or high neutralization number, the askarel is probably an operating hazard." Also, "If the high power factor is not due to these causes, it is probably not an operating hazard except that when the power factor is quite high, it may result In excessive heating of the device in which it is used."
-94-
QZbizi*
|
TOWOLDMON0028682 WATER_PCB-00013151
Since heat resulting from power factor increase of the askarel in most any commercial transformer is negligible compared with heat generated by the core of the transformer, this consideration does not appear important.
If the suggestion were limited to a 2 percent power factor, It would appear low and probably subject to considerable objection. However, when stated as 2 percent or more, the intention and purpose of this suggestion justifies earnest consideration, although In absence of more knowledge, it appears that conclusive answer to this question is not at hand.
However, it should be apparent that when the power factor of the askarel is 2, 5. or 7 percent or higher at 20C. and 60 cycles, and volume resistivity at 100C. is 20 x 10 Ohm-cm. or lower, contamination is present. As it is likely that such a condition can be rectified by simple earth treatment and filtra tion, there should be little question about desirability of doing this purification work to assure the best possible perform ance of the transformer.
Arced Conditions It is fortunate that there seem to be very few cases of significantly arced transformer askarel, as it is difficult to estimate the possible success of reclaiming the fluid. Particularly, It is not easy to lower the free and also the after corrosion chloride levels within the extremely low specification limits for new askarel.
55"
02632?9
|
TOWOLDMON0028683 WATER_PCB-00013152
Treatment with dry earth as usually used to refine contamina
ted askarel, probably will not rectify arced askarel. Special
refinement, including hydrolysis of the spent scavenger material,
water extraction of excess chlorides, treatment; with wet earth,
special drying and finally treatment with dry earth is required.
The following example is considered typical:
During routine testing of a transformer filled with aBkarel,
a short occurred in the winding, and the arc resulted in formation
of easily seen carbon particles in the fluid. The following
shows the ineffectiveness of dry earth treatment and the need
for wet or water treatment to reclaim a sample of this material
in the laboratory.
Passing the damaged fluid through filter paper failed to
remove the carbon. The carbon was removed by filtering through
paper fitted with a one-half inch pad of Attapulgus earth. At
this stage, analysis indicated the following pertinent properties
as compared with the specification limits:
PROPERTIES OF TRANSFORMER ASKARELS
Property
Specification
Sample
Inorganicchlorides
Acidity, mg. KOH/g. Moisture
0.01 ppm. max.
0.010 max. 30 ppm. max.
0.25 PPm.
0.004 75 ppm.
Then 0.2 percent by weight of Attapulgus earth was added and
the mixture held at 90C. and agitated for two hours and filtered.
This reduced the water to 15 ppm., but the chlorides remained at
0.25 ppm.
Another portion of the original sample was treated with 0.5
percent of earth, held at 50C. and agitated for two hours and
filtered. This lower temperature treatment reduced the water to
only 60 ppm. and the chlorides remained at 0.25 ppm.
-96-
0?63?30
TOWOLDMON0028684 WATER_PCB-00013153
At this stage, the electrical properties were determined and
found to be well within specification limits.
Property
Specification
Sample
Resistivity @ 100cC. x 10 Ohm-cm.
100
576
Power Factor @ 100C. and 1,000 Cycles
0.18$
Dielectric Constant @ 100C.
3.8 - 4.3
4.2
The above reclaiming tests were repeated using "wet" earth
which contained 15 percent moisture. Again, the chlorides remained
at the original level of 0.25 ppm., well out of specification.
Then a sample of the askarel was extracted with water, using
20 percent based on the weight of the dielectric fluid. This
reduced the chlorides to 0.15 ppm., and a second aqueous extrac
tion using 10 percent of water was required to reduce the chlorides
to no detectable amount. The excess moisture was then removed
by blowing with dry air and finally filtering through dry earth
and filter paper.
Although transformer askarel is several times as expensive
as mineral oil, the material is not a high cost item. Therefore,
the economies of undertaking work as described above must be
weighed against the cost of new askarel.
In any event a fair estimate of the reclaiming cost plus
packaging, shipment to location for the work, the cost of several
analyses Involved, then repackaging in new containers and cost
of return freight will indicate at least 50 percent of the cost
of new askarel. Accordingly, usually the most practical expedient
is to purchase new askarel to replace the arced material'.
-97-
0263^31
J
TOWOLDMON0028685 WATER_PCB-00013154
CHAPTER 12 DERMATOLOGY AMD TOXICOLOGY
Skin Exposure Aroclors, or askarels, accidentally spilled on the
skin do not cause an acute toxicity hazard, nor will they cause serious Irritation. The materials should be washed from the skin with soap and water. Prolonged skin contact should be avoided. If work clothes become Impregnated with these fluids, they should be removed and washed.
When sampling tank cars, canvas gloves and safety glasses, or goggles, should be worn. No special clothing is required, but the workers' garments should be laundered at least weekly and changed. If Aroclors or askarels are spilled on the clothes.
If accidental burns occur from contact with hot askarels, the burn should be treated the same as any ordinary burn. Aroclor, or askarel, adhering to the burned area need not be removed immediately unless treatment of the burn demands it in which case, soap and water, or repeated washings with a vegetable oil should be used. Accidental contact with the eyes results In painful Irritation, but not permanent damage to the tissues or the sight. In event of such contact, the eyes should be flushed with a large amount of water for at least 15 minutes. The patient should then be referred to a physician who will treat with an ointment to soothe the eye.
"53-
0263232
TOWOLDMON0028686 WATER_PCB-00013155
Exposure to Vapors
Vapors from hot Aroclor, or askarel, have a degree of
toxicity and should not be Inhaled over a prolonged period
of time. Experimental work on animals Indicates that the
maximum safe concentrations of vapors In work rooms Is in
the range of 0.5 to 1.0 mg. per cubic meter of air. Harmful
amounts of the materials are readily detectable by odor anc
Irritation to the eyes. Usually, people can detect concen
trations of askarels in the amount of 1.0 mg. per cubic meter
of air, which Is the level regarded as the safe work room
limit for an 8 hour day exposure.
Capacitor Impregnations may be done at temperatures as
high as 266F. (130C.). Following impregnation and draining
the chamber, exhaust ventilation should be applied to the
chamber to prevent askarel vapors entering the work room.
Also, when opening a heated capacitor Impregnating chamber,
the workmen should wear a respirator during this short Interval
of exposure.
If transformer askarels are used at temperatures above
125 to 150F. to fill an open transformer, exhaust ventilation
should be provided in the Immediate area.
The many years of satisfactory and safe use of Aroclors,
or askarels, by the electrical industry for impregnating
capacitors and filling transformers has demonstrated the
Industry's ability to handle these fluids without hazard to
the workmen.
It is both simple and in line with "good housekeeping"
and personal cleanliness to exercise the suggested precautions
in all cases.
-QQ-
0263233
TOWOLDMON0028687
WATER PCB-00013156
Vapors from a Severely Arced Askarel Transformer
Experimental data indicate that when askarel is decomposed by an electric arc, insignificant amounts of chlorine and phosgene gas are liberated. The gas is almost entirely hydrogen chloride, which is readily detectable by its odor and its irritating characteristics in even small amounts. Thereby, adequate warning of its presence is provided and significant amounts of fumes would be likely to cause a hazard only in a closed area. Individuals would not voluntarily expose themselves to serious toxic levels of the hydrogen chloride gas fumes.
-100-
0263231*
|
TOWOLDMON0028688 WATER_PCB-00013157
WATER_PCB-00013158
N t'-o" J !II
T A K K. C A n. _ L^,0 _A. D ' K1_G
M/vran. >\7&-1
t~oo Locat'q.n See- 9c SICpT
026323b
|
TOWOLDMON0028690 WATER_PCB-00013159
IS
End Elevation
0?<^38
TOWOLDMON0028692 WATER_PCB-00013161
WATER_PCB-00013162
WATER_PCB-00013164
WATER_PCB-00013165
Scale- 3** l'-0`
Rc.rejtence. Dkaw/nos-
P&Tip0eR. ALGa-6y.pTuAtN-K-dC-anO Material- sbm-bs
PLATFORM or. IZfcoTANK- dC'BT-lS
Monsanto Lhemical Company
PHOSPHATE DIVIStON' ANNISTON. ALABAMA
..
REVISIONS NO. DATE WHBOYM
PLANT
ANNISTON*
TITLE DIPHENYL DERIVATIVES' Vent Tan< F^ I Z60 Sto^a4C. "5hk*
DRAWN BY^'*`lfn(4,l
DESIGNED BYJ'NHP
CHECKED BY J,W.N.P9-Z3*tl APP. BY W | b 5`Z"i-''4 1
BCALE 3'1*6
.
DWG. No. 3C-Q2A3
026 3243
|
TOWOLDMON0028697
WATER_PCB-00013166
WATER_PCB-00013168
9*?9?0
7""
TOWOLDMON0028700 WATER PCB-00013169
TOWOLDMON0028701 WATER_PCB-00013170
TOWOLDMON0028702 WATER_PCB-00013171