Document 5LaDrEwmOx43360RRmbww6BrR
bcc:
]
AG Eades GR Buchanan 2nd Street - Don R NEW YORK - H Gilbert NEW YORK - WE Schalk/AL Klemm
Juno 1, 1965
Mr. Carl Raman Lever Brothers 390 Park Avenue New York, New York
.
Dear Carl:
I am sorry we missed seeing you during my recent visit with Henry Gilbert in New York. However, 1 will look forward to stopping by next time in town.
Henry indicated you had come questions regarding stress cor rosion cracking. He asked me to write you directly. As 1 look back over the early stages of your Hammond project, 1 remember we went through this Game question in June of 1962. Based on an additional three years' experience Carl, I again will optimistically state that this type of failure should not be a problem in. your new system with THERMINOL as the heat transfer medium.
In reviewing the metallurgical failure on a recent visit to your Hammond installation, your personnel there indicated to me . that they were of the conclusion the weld failure was due to poor fabrication, rather than a stress corrosion crack. I do hope ' this is the same information that was relayed to you from that source. You will recall your concern was regarding the integrity of dimple jacketed vessels and I revealed thoro wore many such installations around the country that had operated successfully. This is also true to date.
\
DSW 435098
STLCOPCB4088159
Mr. Garl Raman June 1, 1965 Page 2
J
The entire question of chloride stress corrosion cracking is still somewhat nebulous. This is true even though metallurgists have devoted many years of intensive study to this problem. The results of their studies have given rise to the hypothesis that five items must be present for stress cracking to take place:
1) Local stress condition 2) Presence of chloride ions (cracking has taken place
with the concentration as low as 3 to 5 ppm) 3) Presence of moisture 4) Presence of oxygen 5) High temperatures
All of these things are necessary at one time to cause a stress crack, though the quantities needed are still somewhat question able. Ironically, you can have all of these items present and still not reproduce a crack with identical conditions.
I am sure incidents of stress cracking in THERMINOL systems can be controlled by the following general recommendations:
1) Stress relieve components where possible at 1650?F. Lower temperatures are not effective. This temper-
ature is at the upper limit of the carbide precipitation range, and a low carbon alloy should be specified if there is a tendency toward intergranular corrosion. A second preventative measure is to go to a high nickel alloy.
2) Maintain moisture free and full system by:
a) avoiding water for system cleanout
b) blowing hot, dry air through the system prior
to filling with THERMINOL
.
c) draw a vacuum on the system prior to filling
with THERMINOL
d) install desiccator traps on open vents, and
e) design the system to include a small bypass line
from the discharge side of the pump or of the
heater to the top of the expansion tank (above
the surface of liquid at operating temperature).
This will continually flash off any hydrogen
chloride and moisture in the system.
___
DSW 435099
*
STLCOPCB4088160
-y
/
Mr. Carl Raman
June 1, 1965
Page 3
....
.......
3) Most important, Monsanto1 s system design recom mendations should be followed to prevent thermal stress of the heat transfer liquid.
It should be remembered, Carl, that although THERMINOL is a chlorinated material, the chlorine is tied very tightly to the biphenyl molecule. Ionizable chlorides can only be formed by overheating the fluid. .
Perhaps the best way to alleviate your concern is for you to dis cuss this with American Hydrotherm. I understand they are supplying the heater for the new installation. They have designed installations utilizing THERMINOL, where stainless steel is in contact with the heat transfer liquid. Also, it would be excellent for you to contact Industrial Process Engineers in Newark, New Jersey, specifically Sid Feldman, who has designed many dimple jacketed stainless steel vessels for THERMINOL application.
\ Also, Monsanto has at least eight stainless installations within our own manufacturing complexes and, to my knowledge, they have not manifested a stress crack even though some have been in operation as long as fifteen years.
I do hope I have made a contribution toward lessening your con cern over the cracking problem. However, I wish we could be more profound about the subject. I hope someday this whole problem will be solved. Considering the time and effort being placed on the question of stress corrosion cracking by the International Nickel Company, the nuclear power industry, and others, I am sure it will be solved. For the time being, Carl, our only recourse is control over the items listed before and good design and operation of the THERMINOL system. You know you can count on us to help;in anyway we can, including review of the design and continuous surveillance of the operation. I hope you will continue to call on us at every opportunity.
Cordially,
S. Shaw Market Specialist Functional Fluids
jf DSW 435100
** .
STLCOPCB4088161