Document 5L6KG2d9GDezgvo9j7N839bN4

St. Louis Research Report No. 1306 Work Completed: March 15, 1955 Reed, in Library: August 26, 1955 cT PINAL REPORT ON AROCLOR 1248 AS A HEAT TRANSFER MEDIUM IN A LAMONT FORCED CIRCULATION HEATER Job No. 2-02-750.01-2957 Monsanto Chemical Company Organic Chemicals Division St. Louis Research Department Work done by: A. M. Ellenburg Written by: , A. M. Ellenburg 0690A30 HARTOLDMONOOQ5136 DISTRIBUTION OP REPORT NO. 1506 1. File 2. Mr. A. M. Ellenburg 3. Mr. H. K. Nason - File 4. Duplicate File 3. Circ. Assoc, and Asst. Res. Dir. - Safe Deposit 6. Mr. p. G. Benignus - Organic Sales 7. Dr. L. L. Fellinger - Organic Engineering 8. Monsanto Chemicals Limited - England 9. Monsanto Chemicals Limited - England 10. Extra 11. Extra 12. Extra ,1 f' 1 : I! \ This report contains confidential information which is the property of the Monsanto Chemical Company and which shall be disclosed only to duly authorized persons. The recipient is held accountable for the filing and safe custody of the report, which must be returned on demand. 0690431 HARTOLDMONOOQ5137 TABLE OF CONTENTS Page No. INTRODUCTION ....................................................................................... 1 SUMMARY .................................................................................................. 1 CONCLUSIONS ..................... 1 RECOMMENDATIONS ... i ... ................................................................. 1 PATENT STATUS ..................................................................................... 1 REFERENCES ............................................................................................ 2 EXPERIMENTAL WORK ............................................................................ 2 A. Equipment ............................................................................ B. Analytical Results on Aroclor Samples .............. 2 3 DISCUSSION ............................................................................................ 5 MATERIAL SPECIFICATIONS AND ANALYTICAL PROCEDURES ... 6 TOXICITY AND HAZARDS .............. 7 ACKNOWLEDGEMENT ................................................................................. 7 APPENDIX ................................................................................................ 7 Table I - Thermodynamic Properties of Aroclor 1248. Physical Constants Figure I - Viscosity Change in Aroclor 124G on Heating in a Forced Circulation Lamont Boiler. Figure 2 - Anticipated Life of Aroclor 1248 When Used at 600F. 0690432 HARTOLDMONOOQ5138 INTRODUCTION Aroc'.or 1248 has been widely used as a heat transfer medium during the past 15 years. These years of experience have indicated that heater design and fluid flow rates have much to do with the success of the Aroclor heater. In 1953, the International Boiler Works Company of East Stroudsburg, Pennsylvania and Monsanto agreed to cooperatively sponsor tests on a Lamont type forced circulation boiler to obtain overall heat transfer coefficients, film coefficients and' maximum operating temperature limits for Aroclor 1248. These data would allow Aroclor heater manufacturers to design more efficient units using Aroclor 1248. SUMMARY An experimental 500,000 BTU heater was built at International Boiler works for the test runs. Two test runs were made at 600F. and three at 650F. All runs were of approximately 700 hours or one month duration. Viscosity of the Aroclor was used as an indication of the degra dation of the Aroclor. At 600F. very little viscosity change was noticed, whereas an Increase in viscosity at 650F. clearly indicated a polymerization of the Aroclor. CONCLUSIONS Aroclor 1248 can be used up to four years at 600F. in a forced circulation heater designed to have rapid turbulent flow in the tubes. Limited use of the Aroclor 1243 can be made at higher temperatures. Viscosity determinations at intervals will be needed to Indicate the proper time to replace the Aroclor. RECOMMENDATIONS The data and experience gained in this test will be incorporated into bulletins and handbooks by the Sales Department. With the design data to be furnished by International Boiler Works Company, an excel lent booklet on the usw of Aroclor 1248 in properly designed heater will be available. PATENT STATUS The use of Aroclor as a heat exchange media is not considered patentable. 0690433 " t HARTOLDMONOOQ5139 2. REFERENCES Monsanto .echnical Bulletin No. P-150. Organic Chemicals Divirion Report on Job No. 117-2060, "Design and Testing of a Portable Aroclor Heating Unit", R. E. Howard, August 1, 1948. ". Phosphate Division Report No. 2210, "Efficiency of Aroclor Heater", L. C. Garrett, November, 1947. EXPERIMENTAL WORK Using the lamont type forced circulation heater described, below, experiments were planned to give continuous operation at both 600 and 650F. for extended periods. As each test progressed samples of the Aroclor were taken to observe the condition of the heating medium. These results are listed with the conditions of each test. A. Equipment An International Lamont Boiler, LCF-5, rated at 500,000 BTU per hour was used in these tests. Full requirements were 5 to 6 gallons of oil per hour to give an input of 690,000 to 850,000 BTU per hour. The heating surface of the tubes is 99 square feet. The boiler tubes are made of No. 85 carbon steel (15 gauge) with 15/16" inside diameter. An arrangement of seven tubes makes two passes through the firebox. Each pass is 27 feet in length to give a total of 580 feet of pipe in the heating area. The firebox temperature was 2000F. and the outside tube wall tempeiiture was measured at approximately 750F. An automatic temperature controller maintained the temperature of the Aroclor 1240 leaving the heater at 600 or 650<>F. as required. A heat exchanger removed heat from the Aroclor so that the .temperature differential was about 50 F. A low flame is automatically used in the firebox until the Aroclor temperature in the return line has reached 150"F. A centrifugal purp, Dean Brothers type with a 5 HP, 1750 rpm motor, was used to pump the Aroclor at the rate of 60 gallons per minute. Orifices in the inlet of the seven tubes from a header Insured a balanced high flow in each tube. 0690434 I HARTOLDMON0005140 3. A flow rite of 60 gpm is equal to 231 cu. in. per second. The cross sectional area of the 7 tubes is 3.62 sq. In. so the velocity of the flow through the boiler tubes Is 64 in per second or 5.3 ft. per second. The Lamont type forced circulation boiler used in these tests is standard equipment of International Boiler Works. Similar design is used for heaters of 4,000,000 BTU/hr. size and larger. 3. Analytical Results on Aroclor Samples Samples of the Aroclor were removed from the heater peri odically during each run for checking the condition of the heating medium. ' Test I: Aroclor 1248 was used in this run at 600F. The system was vented to the atmosphere. Dowtherm and a phenyl silicate had been used in the system prior to the Aroclor run so slight con tamination from these materials may be evident. Analyses of the Aroclor samples in use are as follows: Test I - 600F. Sample No. Date Hours Saybolt Seconds Sp. Gr. at 65/15.5 C. Viscosity at 130' Start 1 2 3 4 5/19/53 5/25/53 6/3/53 6/9/53 6/16/53 0 168 357 504 671 1.394 1.394 1.394 1.395 1.396 66.5 69-1 72.1 74.4 76.8 Test II: The second phase of the Aroclor heater operation was started at 600F. under 30 psig nitrogen pressure. A failure in the cooling water supply caused the Initial run to be halted. For about 20 minutes the Aroclor was heated to 76oF. The Aroclor showed a viscosity increase from 72.8 Saybolt Seconds to 73.3 SUS at 130F. This slight increase was not considered harmful. The test was started again with new Aroclor and sampled as the run continued. Analysis of the Aroclor is given below: Test II - 6oof. - 30 psig Nitrogen Pressure Sample Date Hours Sp. Gr. at 65/15.5C. Viscosity at 130F. Initial 1 2 3 i4 7/29/53 6/5/53 0/12/53 0/19/53 0/26/53 0 168 322 479 547 1.406 1.407 1.407 1.406 1.406 72.4 73-4 73.6 74.0 74 .8 0690435 HARTOLDMONOOQ5141 4. Test J.IJ For this run, the flow rate of the Aroclor was decreased by installing a new set of orifices in the header. Aroclor temperature was maintained at 650F. with 30 pslg nitrogen pressure. Samples were ><?sted at intervals during this run. Test III - 650 F. - 30 psig Nitrogen Pressure Sample Date Hours Sp. Gr. at 65/15.5C. Viscosity at Initial 1 2 3 4 10/7/53 10/16/53 10/21/53 10/25/53 11 A/53 0 216 336 500 668 1.408 1.4o8 1.410 1.4o8 1.409 73.7 61.5 90.6 102.2 117.7 A leak v.as discovered in the condenser at the end of 336 hours, so the exact pressure during the run up to this point is questionable. The leak was fixed and 30 psig nitrogen pressure was applied during the remainder of the test. Test IV: The unit was charged with Aroclor used previously in Test II. The test conditions were the same as Test III except the rate of Aroclor circulation was increased approximately 12#. After two weeks operation it was noticed that the pressure on the system had increased from 30 to 70 psig and at the end of the test the pressure was 90 psig. Test IV - 650F. - 30 psig Nitrogen Pressure Sample Date Hours Sp. Or. at 65/15.5C. Viscosity at Initial 1 2 ) 4 12/23/53 12/30/53 1/13/54 1/20/54 1/27/54 0 168 336 500 668 1.406 1.408 1.406 1.409 1.410 76.3 80.8 88.5 97.B 110.4 Test V; This test was run at 650F. with an Imposed pressure of 125 psig nitrogen on the system. Samples were taken during the run for analyses. Test V - 650F. - 125 psig Nitrogen Pressure Sample Hours Sp. Or. at 63/15.5C. Viscosity at 130P. Initial 1 27 4 18 174 342 510 676 1.407 1.407 1.408 1.410 1.405 74.6 77-7 31.9 37.2 J4.7 0690436 HARTOLDMONOOQ5142 s 11 5. The result 3 of Tests II, III and V are plotted on Figure 1 to show the increase in viscosity versus time. Figure shows the life expectancy of Aroclor 1248 when ' handled properly in a heat transfer unit. The data for this plot are from a Lamont type forced circulation unit located at Crawford Manufacturing Company, Third and Decatur Street, Richmond, Virginia. After one year's operation at 600'F., the viscosity of the Aroclor had Increased to only 8J.5 Saybolt seconds at 130F. It was recommended that the Aroclor be continued in service. DISCUSSION The results of these tests indicate that with a properly designed heater to give adequate circulation of the Aroclor 1248 a very long life of the heating medium can be expected at 600F. At 650F., the plotted data show a more limited life can be expected from the Aroclor 1248. Since HC1 is evolved on heating at the higher temperatures, a condensation to form high molecular weight and more viscous compounds occurs. Therefore, the viscosity increase was used to indicate the ^ condition of the Aroclor. Other properties such as color, specific gravity and acidity are not sufficient to tell the condition of the Aroclor. Heating Aroclor in the presence of iron will discolor the material without affecting its properties as a heat transfer medium. There was little change in the density of the Aroclor used in these tests so density is not sensitive enough to indicate the condition of the Aroclor. Acidity indicates some deterioration of Aroclor, but the limited solubility of HC1 in Aroclor prevents this test from showing any cumulative degradation. Viscosity was therefore chosen to indicate the condition of the Aroclor in a heating system. Aroclor 1248 has a viscosity of 73-80 Saybolt Universal Seconds at 130F. In Test I, some contaminants from previous tests were present so the results are not considered. Test II at 600F., shows very little change in viscosity so that years of life might be anticipated from the Aroclor. Tests III, IV and V were all at 650CF. The greater deterioration is noticed in Test III. During this test a leak in the closed expansion tank allowed the pressure to bleed off, so the exact pressure during the first part of the test is unknown. In Test IV, a change was made in the orifices and pump to increase the flow rate of recirculation by 12$. The pressure on this test was 0690437 HARTOLDMONOOQ5143 6. starter* a' 50 psig with nitrogen, but rose to 90 psig during the test. This pressure was no doubt due to the HC1 .gas released in the closed system. Less increase m viscosity was found in a month's test than in the Tevlous test at 650F. The improved flow rate may have been responsible for the reduced degradation. For Test V, the pressure on the system was started at 125 psig with nitrogen and remained at this pressure throughout the run. The increase in viscosity was noticeably less than in Tests III and XV. The increased pressure may have shifted the equilibrium to some extent so that the Aroclor was more stable. The faster flow rate used in Test IV also continued in this test and contributed to the lower degradation by reducing the time of Aroclor contact w.th the heated tubes. In our opinion 650F. is too high a temperature for continued Aroclor 1248 use. Eventually it will break down to give a liquid which will be very viscous and would not be pumpable at low tempera tures in case of a cold start-up. The most trouble free use of Aroclor 1248 as a heat transfer medium can be obtained by limiting the maximum temperature to 600F. in a forced circulation heater. In addition to the results obtained here on reporting the condition of the Aroclor, engineering data on the use of Aroclor in heat transfer applications is being assembled by International Boiler Works. An engineering handbook is being prepared Jointly by Monsanto and International Boiler Works to enable design engineers to properly design Aroclor heating systems. Monsanto is writing the portion pertaining to the physical properties of the Aroclor 1248 and the chemical characteristics that concern the stability and life of the Aroclor. International Boiler Works is supplying the charts on film coefficients, over-all coefficients for heat transfer, pump per formance curves, pressure drop in various pipe sizes, flow rate selection curves for pumps and thermodynamic properties of the Aroclor 1248. Table I which is included in this report is the thermodynamic chart fo" the booklet. MATERIALS SPECIFICATIONS AND ANALYTICAL PROCEDURES Aroclor 1248 is produced at both Anniston, Alabama and Monsanto, IlllnciB plants. . \ 0690438 HARTOLDMONOOQ5144 7- The standard tests for non-dielectric uses are made to meet these specifications'. Api.arance and Color Colorless to.light yellowgreen liquid; APHA 100 max. Condition , Specific Gravity at 65/15-5C. Acid Number (mg KOH/gm) Moisture (H20) Viscosity at 150F. Clear 1.405-1.415 0.010 Max. 55 ppm, Max. 75-80 SUS Viscosity determinations on the condition of the Arcelor 1248 after use was made by using a standard Saybolt viscosimeter and ASTM 0-88 at 150F. TOXICITY AND HAZARDS The toxicity of Aroclor 1248 is covered in Monsanto Bulletin 0-P115, "The Aroclors". Bulletin P-150 on the Aroclor heater also discusses the toxicity and hazards involved In using Aroclor. The proper equipment to safely handle Aroclor as a heating fluid is also ably discussed. ACKNOWLEDGEMENT Mr. P. G. Benignus in charge of Aroclor Sales has been an able proponent of the use of Aroclor as a heat transfer fluid, h'is efforts in arranging for the tests with International Boiler Works are gratefully acknowledged. Mr. George Stabenow, Chief Engineer, and Mr. Russell Imbt, Jr., Project Engineer, of International Boiler Works have contributed greatly to the demonstration that Aroclor 1248 can be used at 600F. APPENDIX The results on testing Aroclor samples are reported on notebook pages - 99752, 99758, and 99770. dm 11-25-55 A. M. Ellen',urg 0690439 HARTOLDMONOOQ5145 TOMWOPimWXC fBOrWmS or MOCUffl #12*8 TABUS 1 Tapr*ture V. *C. 3? to 50 60 70 So 90 100 110 i:*o l1C3o0 1>0 lt0 1iA70o 190 200 210 220 230 2*n 250 20 pro 21)0 290 300 310 >20 330 >40 31/) >O0 3>7io0 3C9o0o <110 *20 MO 1*0 *1/) *t0 *k7h0o *90 500 1,10 520 630 6*0 660 y*o 570 660 690 600 010 620 630 0 * 10 16 21 27 32 30 *3 5*?4 00 60 71 77 V2 mi 93 1909? 110 no 121 127 132 138 1*3 13* 160 100 171 177 ite 166 193 199 20* 210 210 221 227 232 233 2*3 2*0 23* 2oO 266 271 277 262 288 29J 29? >0* 310 316 >21 >27 2 Enthalpy Dtu/lba. 0.000 2.1 >2 4.681 7.016 10.307 13.134 13.917 18.716 21.331 2.. >62 27.209 30.072 332?..9?3*o1 36.737 Cl .70* **.727 <*7.666 60.6ol 53.651 30.067 59.679 62.717 63.7^1 Oc.6*l 71.927 7*1.029 77.1*7 00.201 63.431 06.397 89.779 92.977 96.191 99.*21 102.607 106.929 109.206 112.*99 116.o5 119.133 122.*7* 17...831 129.204 132.593 135.990 139.*19 1*2.056 1*6.30? 1*9.770 133.2o2 160.762 160.278 103.810 1o7.J58 170.922 174. 502 178.093 101.710 135.J58 183.932 0 p Sp*c. H**t Ptu/lta.*P. 0.2695 0^711 0.2727 0.274} 0.2759 0.2775 0.2791 0.2007 0.232> 0.2339 0.2855 0.2071 0.2867 0.2903 0.2919 0.2933 0.2951 0.29o7 0.2902 0.2998 0.3O14 0.3030 0.3046 0.3062 0.3078 0.3034 0.3110 0.3126 0.31*2 0.3158 0.51r* 0.3)90 0.3206 0.3222 0.3238 0.3254 0.3269 0.3285 0.3301 0.3317 0.3331 0.33*9 0.3365 0.3381 0,3397 0.3413 0.3429 0.3445 0.3461 0.3476 0.3*92 0.3508 0.3524 0.3540 0.3556 0.3572 0.3668 0.3604 0.3620 0.3636 0.3652 Danalty Lba./ou.ft 91.6 91.3 90.9 90.6 90.2 69.6 89.5 89.1 OS.O 88.4 88.1 87.8 67.* 67.0 do. 6 86.2 g5.? 65.6 85.2 8*.8 6*.* 6*.l 83.7 83.4 83.1 82.9 62.6 82.3 61.9 81.u 81.2 60.9 80.6 60.2 79.8 79.4 79.1 76.8 78.5 78.2 77.9 77.6 77.2 76.8 76.4 76.1 75.7 75.4 ft? 7*.* 74.1 73.7 73.4 73.0 72.7 72.4 72.0 71.7 71.* 71.0 M>/.* 12.22 12.19 12.13 12.06 12.03 12.00 11.96 11.91 11.67 11.82 11.77 11.73 11.69 11.6* 11.58 11.53 11.47 11.42 11.38 11.34 11.29 11.2* 11.18 11.14 11.10 11.06 11.03 10.96 10.94 10.90 10.63 10.81 10.76 10.71 10.67 10.62 10.57 >} 10.*8 10.43 10.3? 10.3* 10.30 10.25 10.20 10.16 10.11 >0.06 10.02 9.96 9.94 9.90 9.65 9.80 9.76 9.71 9.57 9.6} 9.38 1:8 Spaolfle Oravlty l.*o l.*55 l.*3 1.445 l.*0 1.432 1.425 l.*20 l.*l* 1.409 l.*0* 1.400 1.493 1.387 1.381 1.375 1.370 1.365 1.359 1.3*6 1.342 1.336 1.331 1.326 1.321 ` 1.316 1.311 1.303 1.300 1.296 1.291 1.266 1.280 1.274 1.269 1.26* 1.259 i-iil 1.2*8 1.2*3 1.237 1.231 1.225 1.220 1.214 1.208 1.202 1.196 l.W 1.166 1.180 1.175 1.170 1.165 1.160 1.155 1-1J* 1.1** 1.133 Abaolut* Vlaoaany CtttlJBl.fi .... ... . ... >60 200 *; , , 66 *7 2! 2* 16 1* U 9.1 l6-.3i !? *.* 5.9 3.35 3.00 2.68 2.38 2.08 }-9<> 1.02 1.C8 1.58 ; ; . i i i 1 . 1.30 1.22 1.15 11..01?5 1.00 0.96 0.91 20.`8aI* 0.80 0.76 0.73 0.71 0.68 1.62 0.60 0.57 0.55 0.55 0.51 0.*9 2-51 0.45 }} 0.*2 0.40 0.39 0.J7 <1 'I r ` f* l, > \ 11-23-65 0690440 I' X *rV# HARTOLDMONOOQ5146 Cr v stH 1 ] 1! i riK p't t i'i SET So ' Hi toil P<M lit u" m 65/15.5*0. i.no crailt> , JOO*C 1.1T0 i R*f THT l 1 v< U,,1<> .25*C. , 1.6*95 ] 1 VlM-USltJ I SurOc; tension 20*Ce 44.2 dyne/cn i S-! ut> 1 i 11 y In "r Insoluble i glycerine : benzene , So I 'jF t 1 1 t > in JA K 1 r` ; S- l,,l- 1 | Hy CC1 Insoluble Very soluble 15 sr/100 Bl et 25 lSoluble h m it i it Monsanto 02-115 1954 Dayton Resort 597i 1949 J.Coll.Sol.1,166 j 1952 Monsanto 02-115 l_1954 It It N It H L!___ n it * n tt n !I j i'Msn ;n' i :i* "F fnioUituI) COC 193-196`C. j Kir- i-w,' y COC Hone H`*at of combustion 1 Hv.-ii. of' IVrniJit ton i/tteiit #*i of fusloii } Ut*nt M-.v. of vap. j Sf-cinc t.-r.i : Cr 1t ica 1 t afjer at.urc ' Critical pressure ! lJ!<5(ien'.U:i c'-iiscant 1RH ! | : ; [ Pounds por /al. i : ________ . : i i 25 r 12.04 r __ i_____ __ J ___ H It -------------- H* M tt 7 i --Da*y---t-o---n-----R---e--port 597:1949 ' Monsanto OP-115 ,1954 | l. 0690441 HARTOLDMONOOQ5147 - "V IS C O S IT Y SAYBOLT SECONDS AT - 3 0 F HARTOLDMONOOQ5148 0690443 HARTOLDMONOOQ5149