Document 4aGgDmmonLKQeDvvD9wkBw47G
PLAINTIFF'S
EXHIBIT
CHV-458
HI Segundo Refinery
o.-u.Ikt a, 1979
\.\;n 27 tiQIUK
Pa;'/; 1 of 3 .'
.
sPEcn'jCA'noN no. .ss-zsth?. ,
,
REFRACTORY LINING FOR REGENERATED CATALYST U-DEND IN `THE FCOU
GENERAL
1.1 Tl\is_ Specification covers requirements for materials, installation, curing, repairing, testing, ami inspecting a cast -1-5/S inch thick monolithic refractory lining. The lining shall contain. -1.2 volume percent stainless steel fiber reinforcement in a -IS inch diameter U-bend (per Drawing SD-120612) and be suitable for 1.100 E on.'.rating temperature. '
1.2 C!ONTRACTOR shall provide and install all materials required following good workmanship practices. All work shall be free from injurious defects.
MATERIALS
. .. .___ .. -
2.1 Refractories '
_ .-
............ '
2.11 2.12.
The "castable refractory" shall he a 130-l-J01h/fl.'! density AST,VI C-l-01
< 1 lass O re I factory lie see US- I 7 K. No subst i tu tea will be ;u:o 'pLed. *'
The "erosion resistant refractory," shall be a l60-1701h/ft^ density
acid bonded refractory Uesco AA-22. No substitutes will be accented.
2. Stainless fibers
....
-
2.21
The stainless fibers shall be AIS1 302 or 304 stainless steel, and. shall bo made by the melt extraction process. Fibers made; of chopped wire shall not be used.
2.22
Stainless fibers mixed into the castable refractory ""shall have an average length of 1 3/o inches, and an equivalent diameter of 0.0 IS to 0.020 inch.
2.23
Stainless fibers mixed into the erosion resistant field joint refractory shall have an average length of 3/4 inch, and an average-diameter of 0.018 to 0.020 inch.
2.3
I iexmesh
..... ...............................
' ''
'
'''
"
rj3 - { 35,
?,,.3\
The hexmesh shall be 3/1 inch thick, 14 gnu;/' AIS1 403-rrr~'idi)U (low
carbon) stainless steel.
2.32
The hexmesh shall be 1 3/4 inches across the Hats, welded or riveted (not clinched), and shall have two "prongs" extending into each hex.
2.33
The hexmesh shall he Eufnel Lance Grid, or COMPANY apnroved
equivalent.
-
CHEVB8 6081
xification No. S'S-2502
Kl Sop-undo lli-finory October S, 1979 l'agc 2 of 8
2.4 Anchors
2.41
Cast able refractory anchors shall be 3M inches tall, 3/16 inch dia
meter, AISI 304 stainless steel V-studs.
`
2.42
Ilcxvncsh supports shall be l4 inch diameter AISI 304 stainless stool
Nelson .studs welded .on 2 inch by 2 inch by hi inch AISI 301 .stainless
flats.
-
INSTALLATION
.
...
3.1 Anchors
. ...
3.11
V-studs for the enstublo refractory .shall be installed in staggered
alternate rows S!I inches apart and oriented per Drawing SK-RCC-
FCC-S.
:
"'
3.12
Nelson studs for the hex mesh shall be installed and oriented per nozzle detail SIC-RCC-FCC-8.
3.13
Nelson and V-studs shall be welded to the inside of the U-bend using F309-15 welding electrodes.
3.14
The entire inside surface "of the U-bend shall be grit blasted to a commercial blast finish (SSPC-SP6), and shah be cleaned of all grit, dust, rust, scale and grease before welding in the studs.
3.2 Ilcxm esh:
__
... ....
--
3.21
The lu!xim\sh shall be rolled the? "hard way" {with the nsis of the roll and axis of the; rivets parallel) and installed in 'aecoTdaiice with Drawing SD-120612.
3.22
The hexmesh shall be welded together and to its supports in accord ance with Drawing SD-120612 using 1-1-309-15 welding electrodes.
3.23
The hexmesh shall be thoroughly cleaned and all grease and oil removed before welding.
3.3 Refractories
'_
. ..
3.31
The entire inside surface of the U-bend shall be cleaned of all grit, dust, rust, scale and grease before applying any and all refractory. All refractory anchors and hexmesh shall be thoroughly cleaned and all grease and oil removed before applying any and all refractory.
3.32
The U-bcnd metal temperature, surrounding air temperature, and refractory temperature shall be maintained between 50. -F and 90F
throughout refractory mixing and application operations.
CHEVB8 6082
peri i'icatiou No. SS-250
El Sogmuio Refinery October 8, 1979 Page ?, of S
3.3 All refractories shall be properly proportioned anil thoroughly mixed in accordance with the manufacturer's instructions and specifications.
a. Each hatch of similar typo refractory shall be mixed to the same consistency and workability established by CONTRACTOR and approved by COMPANY.
1. CONTRACTOR shall submit for COMPANY approval the
ASTM CS60 Ball Jn Hand Test range at which the castable
refractory will be cast.
2. CONTE ACTOR shall ..u'uuit far COMPANY approval :
ASTM Cl Ml Workability Index range at which the AA-2 2
erosion resistant refractory will be rammed.
.
b. Within the manufacturer's recommended water limits, only enough water shall be added to the refractory to achieve the approved application consistency and workability.
1. For the castable refractory, no more titan 20 cups of water shall be added per 100 pounds of refractory without COM PANY approval.
2. For the erosion resistant refractory, no more than 6 cup-; of waller shall be added per 50 pounds of refractory without COMPANY approval.
c. All refractories shall be poured or placed within the manufac turer's recommended time limitations. Refractory not used within tiie recommended time shall he discarded, and not remixed.
' 1. Castable refractory not applied within 25 minutes after the ' addition of water shall be discarded, and not reused. 2. Erosion resistant refractory not applied within 15 minutes after the addition of water shall be discarded, and not reused.
d. Refractory should be mixed only long enough to produce a uniform
mix. Under no circumstances shall refractory be mixed longer
than 5 minutes after the addition of water.
-
-,
e. Only fresh, unused, non-rocovcred refractory shall lie used.
f. Only clean, fresh, nonpolluted water suitable for drinking and free from injurious amounts of organic matter _or other deleterious substances shall be used.
g. Refractory mixers shall be cleaned, and free of any contaminant, before mixing each batch of refractory.
CHEV B8 6083
icei fica lion Mo. SS-2.502
K1 Scgundo Refinery October S, 1979 Page 4 of 8 -
,2.4 Six pounds of clean, oil-free, stainless fibers shall be mined into every cubic foot of castable refractory (1.2% fibers by volume). The stainless fibers shall be screened to breakup knotted fiber and thoroughly mined into the castable refractory to achieve a uniform distribution of randomly oriented fibers.
2.5 The castable refractory shall be vibration cast into each U-ber.d segment in
one continuous operation in accordance with manufacturer's instructions ami
specifications.
.
a. lunch U-'mivl r.eipni'ut shall bo poured as a single continuous cast in". If
more than mie pour is required to iiii|d.!i.e .i U-b.:u.; upnt'iit, the
time between pours shall bo minimised and. shall not exceed 30 minutes.
b. Sufficient vibration shall be applied to the U-borid to achieve a dense:,
uniform casting free of vapor pockets and voids.
c. Casting forms and molds shall be treated or coated to prevent
premature loss of moisture during refractory airing, and to minimize
refractory adhesion to the forms.
-
d. Within 30 minutes after completing a U-bcnd segment casting, all
exposed refractory surfaces shall lie coated with a color tinted curing
compound approved, by tlie* refractory manufacturer.
3.6 The erosion resistant refractory shall be rammed into eacli hex mesh section in accordance with manufacturer's instructions and specifications.
a. Underlying castable refractory shall be clean and free of any contami
nation that would adversely affect adhesion,
h. Sufficient ramming and hammering shall bo applied to the erosion
. resistant refractory in each hoxmesh section to achieve a dense,
. uniform "biscuit" free of air bubbles, pocket and voids, and completely
, filling the hoxmesh.
c. If a batch of refractory should stiffen before placement in the
` hoxmesh, to the point where it is not binding together, the batch shall
be discarded. Under no circumstances shall more water be added or
' the refractory remixed.
d. The erosion resistant refractory shall not be coatc.d with a curing
compound without COMPANY approval.
1
REFRACTORY CURING
. . .. ... .
4.1 All refractory shall be cured and dehydrated in accordance with manufac turer's instructions.and specifications.
4.2 Prior to the installation of any refractory, CONTRACTOR shall provide, for COMPANY approval, a planned curing and dehydration schedule allowing hold times, temperatures, and heating rates. The ..COMPANY approved schedule shall be followed Cor all refractory curing and dehydration.
CHEV B8 6084
Specification No. SS-2502
HI Segundo I'criricr/ Octobers, 1979 Page 5 of ft
4.3 All refractory shall bo hydraulic cured at least 24 hours (or at least -13 hours if the temperature is below 65F) before removing the casing form:;.
4.31
The castable refractory shall bo kept moist throughout hydraulic curing. A fine water (suitable for drinking) spray shall he applied to exposed refractory surfaces and casting forms as necessary to keen tin: castable rou\u:tury moist during hydraulic curing.
4.33
Tho erosion resistant refractory shall not be moist cured without COMPANY approval. Water or water spray shall not be applied to the erosion resistant refractory during curing. Erosion resistant refracr"ry mull not he .,,..i|ed from direct cmif.urt vi* 11 Ike . tuui.i'ih v;.
4.33 . Surrounding air temperatures shall he maintained between 50F and
SO F during all refractory hydraulic curing.
4.34
After removing the casting forms, all refractory shall air dry at least 24 hours before heating for dehydration.
4.4 All refractory shall be thermally dehydrated to 600F at a rate slow enough to
prevent steaming. As a maximim, all refractory shall be dehydrated no faster l h.m l In * following, with additional hold:; as necessary to prevent steaming.
4.41
Heat from ambient temperature to 250F at no more than 25F per hour. .
4.42 Hold temperature at 250lr for at least 12 hours.
4.43
Heat from 2501'' to 600F at no more than 50F per hour.-"
4.44 Hold temperature at 600F for at least 6 hours.
4.45
Temperatures above are curing gas temperatures; not refractory or
metal temperature.
,
4.5 Thu thermal dehydration of all refractory shall be done using only the convection heat of hot circulating gases. No portion of the refractory shall bo subjected to flame impingement or direct radiation at any time during the thermal dehydration.
4.51
Tho gas temperature shall be continuously monitored and recorded, throughout the dehydration procedure with nt least 3 thermocouples, one at the middle, and each cncl of each U-bend segment.
4.52
The temperature difference between thermocouples in a U-bend segment shall be minimized and not exceed 50 F.
4.53
Tho record of the thermocouples' temperatures shall bo given to. tho COMPANY.
CHEV B8 6085
Specification No. SS-2.502
FI St'",undo Refinery October8, 197V Page 6 of 8
4.6 The U-benil mof.nl temperature shall be continuously monitored and recorded throughout the dehydration procedure, with at least 2 thermocouples evenly spaced on each U-bond segment.
4.61
The record of the thermocouples' temperatures shall be niven to the
COMPANY.
5. REFRACTORY REPAIRS
. _ ...
-
5.1 All refractory that dues not meed all the. requirements of this Specification shall be replaced or repaired, at CONTRACTOR'S `xpenso, in accordance with this Specification, includin';, refractory mixing, application and quality control.
5.2 CONTRACTOR shall provide for COMPANY approval a planned curing and dehydration procedure for all repaired areas. Repaired areas shall be cured and dehydrated in accordance with the COMPANY approved procedure.
5.3 Small voids and large cracks in the castable refractory shall be chiseled out to
sound adjacent refractory, and repaired with rammed llesco AA-22 or COM
PANY approved equivalent.
'
5.3 1
Repair areas less than II.' inches deep or covering less than GO square inches shall be considered small.
5.4 Moderate sined voids and defective areas in the castable refractory shall In completely removed down to the U-bend exposing at least one entire V-stiul.
5.41
The sidewalls of the repair area shall he angled outward 15-25 degrees such that the repair area adjacent to the U-bend is larger than the outer surface of the repair area.
5.42
Repair areas with only one exposed V-shtd shall he rammed with fiber reinforced Resco AA-22 or COMPANY approved ecpnval^nt.
5.43
Repair areas with 2 to 4 exposed adjacent V-studs shall be rc-cast with
fiber reinEorced castable refractory.
'
5.44
Repair areas with more than 4 exposed adjacent V-studs shall be considered major repairs.
5.5 Major voids and defective areas in the castable refractory shall be completely removed down to the U-bcnd in a band 360 degrees around the. .U-bend exposing at least two rows of V-studs. The removed refractory shall be re-cast with fiber reinforced castable refractory.
5.6 Defective erosion resistant refractory biscuits in the hexmesh shall be completely removed, and replaced with rammed erosion resistant refractory.
CHEVB8 6086
ci l ii11 ion Mo. SS-25-02
Kl .Si-,;undo Refinery October 8, 1979 Page 7 of 8
QUALITY' CONTROL
6.1 Testing
6.11
F-efraeiory studs:
All Nelson and V-stud attachment welds shall he hammer tested. All loose studs, bent over studs, ami studs with cracked or partial attachment welds shall be removed, replaced, and retested.
6.1 i'.uCr iiln-y Mi:::
_
a. Each lot of refractory shall be pretested to determine the amount of water necessary to obtain the COMPANY' approved consistency and workability. This water content shall be reported to COMPA NY'' (as cups of water per 100 pounds of refractory) along with the refractory lot identification.
b. For every batch of refractory mixed, the total amount of water (in cups) and refractory (in pounds) added to the mix shall be reported to the COMPANY'' along with the refractory lot identifi cation.
6.13
c. Every batch of mixed refractory shall be ASTM C&60 and ball-in
hand tested for proper consistency and workability before casting
or ramming.
"
Refractory Cure:
,a. Etrch lot of refractory shall be pretested in accordance with ASTM C26S to determine its modulus of rupture with the speci fied reinforcing fibers. All refractory lots with an average
modulus of rupture after thermal dchyration less than 1500 psi, or a single test valve below 1000 psi shall be rejected and not used.
1. CONTRACTOR shall provide COMPANY' certified. ASTM C26S test results for each thermally dehydrated test brick from every refractory lot tested. The test report shall .also
. . _ indicate the refractory dry weight (to the nearest 100 'grains) of the test batch, and the amount of water added (to
... the nearest milliliter).
2. The ASTM C268 test hatch of refractory shall he mixed using the amount of water necessary to obtain the COM PANY' approved consistency and workability.
3. The five thermally dehydrated ASTM C263 test bricks shall be dehydrated at i.200F rather than one of the ASTM C263
heating sclrcdulcs.
..
CHEVB8 6087
ipocificalion No. SS-2502
El .''".uailo Refinery October S, 1979 Pago S of 8
-1.
The five, hydraulically cured oe.ly, A STM C268 lesd bricks shall be
clearly identified with the refractory lot number, and provided to
COMPANY for information only.__
_
f'Tlie cold crush strength of each batch of mixed refractory shall be
f_. ` rioter in in d in ao-nrdnnoo with VSTM C133 modified as follows:
.
1. A 2 inch by 2 inch by 2 inch cube Lest specimen shall he used instead of thu ASTM C133 specimen.
2. Nine specimens shall'bo tested from each batch of refractory ii P '< >' 11.
The r ..iciory :.p.-ei ;,i-sis .T ill In- i:y.!.-.!''..illy nr -I ' Jr-. j : and thermally dehydrated 18 hours at 25()',li' before testing. 4. CONTRACTOR shall report all cold crush test results (to the nearest 10 psi) to COMPANY, along with thu required water content report. In addition, the location of.each hatch within the U-bentl segments shall be reported to COMPANY.
All refractory batches with an average cold crush strength less than 8000 psi, or a single test valve below 50.00 psi shall be rejected and replaced.
6.2 Inspec tion
6.21
COMPANY inspectors and representatives shall have access to CON
TRACTOR'S facilities to inspect the refractory during all phases of installation, including anchoring, mixing, application, curing, and test ing. -
6.22
CONTRACTOR shall visually inspect all exposed refractory, after it has been cured and thermally dehydrated, for cracks, voids, r.pallin;;, and unbounded material.
a. Cracks deeper than one inch or wider than 1/16 inch art: unac
ceptable, and shall be repaired.
b. Voids and holes deeper than 3/16 inch or wider than '/ inch are
unacceptable, and shall be repaired. .
c. Any and all spalling or blistering is unacceptable, and shall he
repaired. .
_
d. Unbounded or soft refractory more than l/o inch deep is unac
ceptable, and shall be repaired.
e. Erosion resistant refractory more than 1/16 inch below the
hexmesh edge is unacceptable, and shall be repaired.
f. The refractory radial mismatch between adjacent U-bend seg
ments shall not exceed 1/8 inch.
g. Segregation or preferential alignment of "he reinEorcir.g fibers is
unacceptable, and shall be repaired.
CHEV B8 6088
fV-<SCAyQ K`CTrRAClo <V
F~-l(L-r^ 3Z> Jf'/7~~S
ECC^
CHEV B8 6089