Document 3eLgKRzLkJde633yN9YQ6qakO
MONSANTO CANADA LIMITED PROCESS TECHNOLOGY - PLASTICS
To: Mr. J. Keletx K-66-223
Subject: TECHNICAL SERVICE LABORATORY SUPPORT - PLASTICIZER STATUS REPORT - January - June 1966
Report submitted by: H. Jongsma DATE June 30, 1966
Distribution:
Mr. E.H. Toombs Mr. J. Bagnall Mr. J. Darby - St. L Mr. H.R. Ford - St.L Mr. W.G. Hatton Mr. R.S. Trump Mr. A. Vendette
'copy
for
OUTLINE:
MTS-66-13-1 Dec. 27/65 MTS-66-13-2 March 17/66 MTS-66-13-3 March 25/66 MTS-66-13-4 April 5/66 MTS-66-13-5 April 18/66 MTS-66-13-7 May/66 MTS-66-MTL-8 June 18/66 MTS-66-13-9 May 11/66 MTS-66-13-10 May 18/66 MTS-66-13-11 May 30/66 MTS-66-13-13 June/66 MTS-66-13-14 June 19/66 MTS-66-13-15 June 20/66 MTS-66-13-16 June 21/66
l.,.-
MTS-65-13-46 MTS-65-13-54 Training Program
DSW 587747
STLCOPCB4093083
MTS-66-13-1: Data stu cs - Dec. 27/65 Job No.: 06-13-7799
.
.
Request: Prepare data covering the following plasticizersmade by Mocan but not by the Organic Division:-DOZ S1165 S1171 DBS S1185 S1110
A. For sections "General description" and ''Properties" the following
will be presented: chemical type; chemical formula; molecular
weight; appearance, acidity; color, moisture, odor, specific
gravity, weight per 1 Gal, refractive index, freezing pt, pourpoint,
boiling-range, flashpoint, viscosity @0C, 25C and 98.9C, Assay.,
Solubility in water. General solubility, D.C.R. Heat Stability.
The pourpoint, heat stability, boiling range, flash point, refractive '
index, odor, moisture, color, acidity, appearance, viscosity at
25C and 98.9C., Assay (GLC and U ester content data have been
collected. All the test procedures followed were checked and
compared with the MC.- procedures by contacting Mr. J. Darby and
Mr. S. F. Joyce.
^.
B. For section "Performance in PVC Sheet11: The following tests have been scheduled where applicable: Shore A hardness, tensile, elongation, modulus, low temperature flexibility, volatility, water extraction, kerosene extraction, brittleness, migration, heat stability, V.R. and IR. The above tests are to be carried out on three basic formulas 43 PHR, 67 PHR and 100 PHR where applicable. A general outline on typical electrical screening formulations, 105 formulation and suggested formulations for volatility, Tf and extractions were sent to us by Mr. C. D. Bias and were discussed with Mr. S.F. Joyce. A concise summary of the specific formulas for each of the above plasticizers still has to be completed before more work can be scheduled on each of the above tests after approval by M.C.
C. For section "Performance in Plastisol formulations": Scheduled viscosity at 23C, 40C and 50C (Initial, 1 day, 7 days and 14 days) for 65 PHR. Several orientating experiments have been carried out, varying the PHR, R.P.M, number of spindle and type of Brookfield used as dictated by the viscosity of the plasticizer to be studied. As a result a detailed suggested procedure will be sent to M.C. for approval; in an effort to collect data based on conditions which are as close as possible to the condition's used by MC.
MTS-66-13-2: - dated March 17/66
Request: test 75/25 DIOP/HOP V.A. Tiles to replace 50/50 D10P/S-160
' Customer: Dominion Oil Cloth. The G.L.C. analyses were carried
out here. Mr. Orem (St. L.) commented that the proposition was
not competitive.
..
DSW 587748
STLCOPCB4093084
MTS^-66-13-3 March 25/^.6 Export (MCAL) of S1170
Request:
run brittleness test on every batch plus composite, including heat ageing on composite. Quality Control reported that every batch for MCAL was tested for brittleness and was found to be within specifications for release.
MTS-66-13-4 Green plastisol, Bennett Ltd. Apr. 5/66 Job No: 06-13-7848
Request:
Run G.L.C. and prepare similar blend. The results have been reported and a one gallon sample was prepared for customer, consisting of Opalon 650 (32% by wt.) and D10P (68% by wt.). which had very close rheology characteristics to the green plastisol supplied (with 70% of a plasticiser with D10P as the nearest equivalent).
MTS-66-13-5: D1DP., Bay Mills Ltd. - April 18/66
Job No:06-13-7869
'
Request:
Customer experienced severe and they investigated every Moisture determinations and facilities were requested.
pinholing throughout their product possible cause of their problem. comments on the Mocan D1DP storage
"v-
Action
taken:
The required data and information was reported. The moisture content of the D1DP sample supplied by the customer was only: 0.0417o "VhichLis well within specification
The Mocan storage system is adequate to keep the products within mdsture specifications. Flintkote requested
fusion data on DOP, Sp60 and DCP. The fusion points were reported (being 127, 89 and 130C respectively) and the effect of Sp60 additions on the fusion point was shown.
MTS-66-13-7 Ailed rubber requested rheology data and identification of a
lacquer.
A report was issued, after further consultations with M.C., on the
rheology data.
Also, the composition and suppliers of a supplied sample of a nitro
cellulose lacquer was reported -
Resin(Acrylic type)
.
20%,
Solvents: Methylene chloride ................... 45%
Toluene ............
25%,
Cellosolveacetate .................... 10%
M.T.S.-66-MTL-8 - June 8/66 Job No.: 06-16-7090
Cancelled
MTS-66-13-9 May 11 1966 - Monsanto (Oakville). Request: Investigate plasticiser odor problem on D10P/D1DP/S-1160/DOP.
-2-
DSW 587749
STLCOPCB4093085
Action taken: Odourless DOP was recommended.
MTS-66-13-10 May 18 1966. Job No.: 06-13-7897
.
Run Low temperature characteristics and shore A hardness on off-grade DiButyl Azelate; DOZ, DOA and DOP (as standard).
Due to unavailability of steam, the moulding will be done in Oakville. The compounds required have been sent. The testing will be done here upon receipt of the slabs.
MTS-66-13-11 - May 30/66 - Flintkote Job No.: 06-13-7882
Request: run a GLC.
Analyses have been carried out and results were
reported: 15 to 207o: Fatty Acid Esters.; 85-807o of D.O.P.
(607o) and D1DP (407o) . Upon request more work will be done.
MTS-66-13-13- Mocan Oakville - Mr. G. Rundans
The results of the identification of a red 004 gauge film have been reported:
DNODP
507o
DOP
107o
S-140 - 407o
I
MTS-66-13-14- DOP odorless - Cont. Can. June '9/66 Job No.: 06-13-7888
Prepare a 4 qts. odourless DDP food grade sample. The sample supplied by the Plant Lab is not odourless and was not accepted by MTS. One gallon and one quart of odourless DOP was shipped from M.C. St. Louis but they have not arrived yet. The samples are being traced.
MTS-66-13-15 - June 20/66-Reliable Toy - Mr. Markiewicz Job No. 06-13-7898
Request: Replace a 907o-107o blend of BDP and Howflex 3030 by a monomeric plasticiser giving an equal hardness and ultimate elongati.on.
Action:
After a telephone conversation of Mr. J. Keleti and Mr. Markiewicz a 1 IG sample of D0Z has been sent to them. We just received samples of Reliable Toy - vinyl balls and of vinyl balls made by their competitors. We reported that Howflex 3030.. is similar to our SHOO. Identifications and more work is underway.
MTS-66-13-16: - June 21/66 - Vinyl Fabric - Daly Morin Job No: 06-13-7899
Customer is having problems with tackiness and the gloss of vinyl fabric.
3 DSW 587750
STLCOPCB4093086
Also with applying flexible vinyl backing problems are being encount ered. Mr. D. Goodwillie has been requested for samples, formulas, and more details.
,
Feb. 14, 1966 Proj. No.: 06-13-7811 General Wire and Cable requested D.C.R. studies on DOZ-E and DlDA-E at time of manufacturing and after storage. The results have been reported.
The requested D.C.R. value of the 50/50 blend of the stock on hand was 3.2.
Requests 65-13-46 & 65-13-54 (Job No's 06-13-7741 & 06-13-7783) General Wire & Cable requested stability studies on D.O.P.-E.
Request: DCR stability was to be improved to meet customers requirements.
Action:
During a 10 week period studies were carried out on IR. Also VR, DCR, G.L.C. tests.and the effect of time were studied. The DOP-samples examined were:
Regular DOP-E - Lot 15125 DOP taken from tank 15.7 DOP-E from Shawinigan Chemicals
Aged and exposed DOP Fresh DOP - S/T6
(which was Mocan-analysed
being D10P) .
>v.
as
Also in consultation with M.C., Mr. C.D. Biasj|*it was reported that the
V.R., D.C.R. and IR results were normal and that our DOP is of good quality and compares well with competitors product.
Training of Sylvester Ko
The training as outlined in the May 2, 1966 - memo (K-66-188 which com bines carrying out the MTS request 66-13-1 and some other plasticiser requests with training on the plasticisers) was carried out from May 2May 17.
The Opalon 650-A6-project for Northern Electric combined training in the P.V.C. area and actual quality follow-up untill the present.
Starting June 13 duties in the area of filing and organization were included also. Mr. S. Ko is to be further trained in Springfield on the P.V.C. testing procedures which include the procedures with the Brabender.
The remaining plasticiser tests of a second training program as mentioned
in K-66-188 and the remaining PVC - Polystyrene test methods to be demon
strated during a third program will follow as soon as possible.
-
H. Jongsma
4 DSW 587751
8k
STLCOPCB4093087