Document 3QRQkVDRGdaqmwwNvy9xLR7qx
seMaaSaSSBi
Specification Data
Highest Recommended Service Temperature
Pyrometric Cone Equivalent
Weight Slap Troweled: As Placed Oven Dried at 220F After 5-Hr Firing at 1750F
Weight Gunned: As Placed Oven Dried at 220F After 5-Hr Firing at 1750F
'.rushing Strengths After 5 Hours Firing at:
220F 1200F 1750F 2000F 2200F 2400F Linear Change After 5 Hours Firing at:
1200F 1750F 2000F 2200F 2400F
3X
3000F 33 (3173F)
148 pcf 133 pcf 130 pcf
153 pcf 142 pcf 140 pcf
570 psi 700 psi 790 psi
___
1040 psi 2390 psi
0.0% 0.0%
-0.2% -0.2%
STD.
2400F 16 (2669F)
132 pcf 116 pcf 110 pcf
134 pcf 124 pcf 118 pcf
1350 psi 1070 psi 1130 psi
--
1480 psi 2870 psi
-0.1%
-0._4%
-0.6% -0.4%
The figures given in this table are average values obtained in accordance with accepted test methods.
LW.
2000F 14(25520
104 pcf 69 pcf 65 pcf
117 pcf 76 pcf 73 pcf
275 psi 338 psi 400 psi 461 psi
--
--
-0.3% -0.6% -0.8%
-- --
C-2 Cement
2300F (2608FI
'40 pcf 126 pcf 120 pcf
142 pcf 134 pcf 128 pcf
6200 psi 4700 psi 2600 psi
-- --
--
-02% -02% -0.5%
-- --
MEAN TEMPERATURE, F 600 800 1000 1200 1400 1600 1800 2000
3X - - 4.10 430 4.68 5.40 635 7.68 Std. - 3.89 3.95 4.05 424 4.57 5.09 LW. 1.42 1.52 1.64 1.76 1.89 2.01 -- --
C-2 - - 3.40 3.50 3.80 4.30 5.10 5.90 conductivity: btu IN. PER SO FT PER F PER HR
3X Blazecrete Standard Blazecrete LW. Blazecrete C-2 Refractory Cement
Pounds required for 1 cu ft
130 (slap-troweling) 140 (gunning)
110 (slap-troweling) 118 (gunning)
65 (slap-troweling) 73 (gunning)
120 (slap-troweling) 140 (gunning)
Packaging 100 lb bags 100 lb bags
80 lb bags 100 lb bags
ET-000090
infiAn Insti/afinn fnr Fvarv Pnmmarrial and Industrial Pirrnnsa
57
8C42