Document 3N0xMqJMRkwxaKJDzbLy2xX5J

Cummlng Paton - General Offices February 11, 1969 PLASTICIZER SALES CALL REPORT FILE E. H, Fording - NEW YORK R. N. Brell - NSW YORK J. R. Darby - JFQ RESEARCH M. W. Farrar - JFK' RESEARCH J. D. Wright - JWRIG W. F. V/aychoff A.U.M. Coaker - JFQ RESEARCH VISIT TO: UNITED RESINS Brooklyn, IS. Y. DATE: February 3 1969 FOR UNITED: Nr. Smith, Chemist Harold , Purchasing FOR MONSANTO: R. N. Brell C. Paton DETAILS: /YWe Pacr-icat/oa/ 1. Bind; Specie; in Aroclor 5460 JLWe told Smltty fchat_^yE-afort- from AroclQS-5460"were being hampered because the filters were, being dissolved in the high temperature line between dies till at ion unit and f`laker. nMr wottltTSontinue tmd-GHx) Ties also designing our now plant to eliminate `this problem. CV ^ Aroclor 5460 Viscosity One of United*a customers has complained that the viscosity of the hot melt has varied by a.3 much as 3500-5000 cps over the past 6 months. Vie gave Shitty viscosity vs. temperature dp.ta for Aroclor 5450 and indicated that even as low as 120JC it was impossible for A-5460 to be the contributing factor. We said more consistent results on the hot melt might be obtained by running viscosities at 140-150C. 3. Lot-/ Color Aroclor 5460 We Introduced low color Aroclor 5460 (NPA<1). We indicated that this was laboratory preparation and that commercial ization was about i year1 away and dependent on customer acceptance so that volumes sufficient to Justify production could be guaranteed. A price of 20-21 cents/lb. P.O.B. Anniston was indicated. Smitty promised an evaluation because he does get requests for a white to colorless hot melt adhesive. It turns out that Piceolyte 370 (30,2/lb.) is used Jv.3t nou. 0357860 &> 2- 4. Uniform Color United haa been receiving Aroclor 5460 which Is not uniform In color. The darker flakes are "poorer In physicals" than the lighter flakes. We told Smltty that we hoped to Improve color uniformity now that a new flaker had been Installed. 5. FDA Approval Because of the delay In getting FDA approval United's largest customer has switched back to a vinyl acetate ad hesive. Although this Is for tying the end3 of bread wrappers and it could be argued that this doesn't need FDA approval, the customer want3 to play safe. The customer wants to go to hot melts because he has Installed equipment although he has yet to appreciate the Importance of viscosity-temperature relationships. He can't under stand why he can't get the same results be hi3 temperature 275 or 375F. 6. Competition to Aroclor 5460 The competitor to Aroclor 5460 considered best by Smltty is Piccolyte S70. (it is lighter colored than A-5460, FDA approved and costs 30 cents/lb. It Is on allocation. United is x'estricted to 6?/$ of 1963 purchases). S70 is B-plnene resin and B-plnene is decreasing In availability. Plcco are promoting o,-pinene resins as replacements but according to Smltty they are poor film formers. The best hot molt formulation -- again per Srnitty -- 13: Elvax 260 Piccolyte S70 24 48 24 This is also DuPont's recommendation. Srnitty believes that Aroclor 5460 is Just as good if it had lower color and FDA approval. Smltty has just submitted 3000 lb. of hot melt where Aroclor 5460 ha3 replaced Piccolyte S70. Customer reaction should tell us if we're as good. Wingtack 95 is not considered good by Smltty in spite of its cost (15-16^/lb. F.O.B.). The odor is very poor. Elvax 260.is considered an excellent EVA resin. 7. Carpet Backing Adhesive Smltty said this market was all Stein Hall at present. (Stein Hall told U3 DuPont is also involved). We know that Stein Hall uses' EVA plus ' a. terpene resin at around 9^/lb. 0357861 TOWOLDMONOQ57602 '3- 8. Amorphous Polypropylene Amorphous PP hot melts are used In such applications as laminating sisal reinforced tapes and excelsior pad3. Previously asphalt was used but it has poor low temperature properties and softens under moderately high temperatures. We suggested Hontars -- in particular -;):9 -- for P.P. I think v/e will have to determine compatibility to arouse Interest. Eastman and Avisun are said to have the best amorphous P.P. 9. Paeon Packaging United has encountered a hot melt they can't match. A bacon package has a hot melt film at the two ends. After packing the flaps are sealed but they heat seal in 2- seconds at anywhere between 275 - 400oJ?. The hot molt marts at 180F. but smokos at 290F. Five R.M. suppliers have analyzed the competition'3 hot malt with 5 different results, vis. (l) opoxy/polyethylene (2) polyetliyleno (3) no wax (4) poly3lt!o/jSVA/'.;ax, etc. We were given a sample and our suggestions are welcome. ACTION: 1. (Mfg.) Eliminate black specks from Aroclor 5460 a3 soon as possible. 2. (luIP) Follow up on low color Aroclor 5460 evaluation in 4-6 v;eoks time. 3. (Mfg.) Investigate means of producing Aroclor 5460 with more uniform color (i.e. absence of dark flakes scattered through bag). 4. (Product Group) Obtain sample of Piocolyta S70. 5. (Research) Include S70 In EVA/A-5460 evaluation program. Note remairks on Elvax 260. 6. (Research) Determine compatibility of Montar 1, 5 and 9 in Avisun amorphous P. P. 7. (Product Group) Write -work request to Research on bacon package hot melt. /es , C. Paton TOWOLDMONOQ57603