Document 3JG5GJeKbo9NbjDNwd5107Gry
t ''
(seif)
CORRECTED COPT
Lab. Report No. 740300
October 6, 1970
Dusting Test Conducted on ' Zonolite Mono-Rote Fireproofing Material
. tf, R. Grace & Co.
Construction Products Division 62 Whittemore Avenue
Canbrldge, Mass. 02140 Attn: Mr. Walter Payment
Research.Dept.
.J. N. Schoenberger Director, Physical Sciences Division BOWSER-MORNER Testing Laboratories,Inc.
Test Report in Accordance MIL-STD-831
10037912
BOWSfcR-MORNER Testing Laboratories, Inc.
ADMINISTRATIVE DAT
CS020
PURPOSE OF TEST
To determine If exposure to a high-velocity airstream will cause erosion or dusting of the Zonollte-Mono-Kote. ' :
Construction Products Division 62 Whittemore Avenue ' Cambridge. Hassachusettes 02140 v *'
,'f-v*7
,- ' '' ;
Zonolite Mono-Kote Fireproofing Material
DRAWING, SPECIFICATION OR EXHIBIT:
QUANTITY OF ITEMS TESTED: Three (3) Pans
DATE TESTS COMPLETED: September 19, 197C
TESTS CONDUCTED BY: The Staff of The Physical Sciences Division Bowser-Momer Testing Laboratories, Inc.
DISPOSITION OF SPECIMEN: Retained by Bovser-Morner Testing Laboratories, Inc. pending instructions from Client.
Lab. Report No. 740300 -i-
10037913
BOWSER-MORNER
Testing Laboratories, Inc.
( b(:21
,XK^':'':' . , SECTION I -i RESULTS OF TEST
CORRECTED COPYFACTUAL DATA
______ ..
. ,
: '
v-^tr':
Folloving-aretheresults obtained during testing of the sample Zonollte Mono-
Rote Material. yTests were conducted as specified in Appendix Bt using the equipment
described ia'Appendlx A.';
.M-y .
. > ' X--
I*}5* V-
'
SS#?3 ^
;.
No dusti could be] detected using the method of iso-kinetit sampling.
.tit
M;-. :
:
; ?'&
v
The aaotmtsfof^dust detected were extremely small, and are regarded by this
laboratory
the band of weighing.errorfThe amount of dust|fomdi>? ]
V,vf' downstreaa froiifthe^Mono-Rote could not be distinguished from the aublent' dust
"level.i: r^S.-yviVV-'/VY '
A microscopic examination of the filter surface revealed no particles which could be definitely-identified. Under this examination, at a variety of magnifi cation powers, the appearance of the upstream filter was virtually identical to
that of the downstream filter.
r
I
*;
10037914
CORRECTED COPY
TEST EQUIPMENT
Following is a description of Che test equipment used In conducting the Dusting Test on the sample Zonolite Mono-Kote.
A wind tunnel designed and fabricated by Bowser-Morner Testing Laboratories, Inc. was used to provide the 50 mph air velocity over the Zonolite samples.
The tunnel consists of an ILC Electric Ventilating Co. Model BC-40 squirrelcage blower driven by a three H.P. U.S. Varidrive Unit, Model VEU-CH, driving air through a 18" high X 12" wide tunnel which tapers down to a 6" high by 12" wide section at the Zonolite samples. Furnace filters were used to filter ambient air at the Mower inlet.
Velocity was measured by a 1/4" O.D. Ellison pitot tube and 0-2" H2O inclined draft gage.
Sampling was accomplished using a Bell .& Cosset 1/4 HP vacuum pumo, two 10 liter/ minute Mllllpore Corp. limiting orifices, four Ashcroft 30" vacuum to 150 psl Bourdon tube gages, two Bowser-Morner Testing Laboratories, Inc. filter holders, and a number of Mllllpore Corp. AAWG 04700 cellulose acetate surface type filter membranes, 47 mm. in diameter.
Filters were weighed on a Sartorius 0-200 gram balance with .OODlg smallest divisions.
f 1
Lab. Senort No. 74DTOO -4-
10037915
BOWSER-MORNER Testing Laboratories, Inc.
Ms,
TEST PROCEDURES
Following Is a description of the test procedures used In conducting the Erosion Test on the sample Zonollte Mono-Kote.
Three 10" X 13 3/4" X 2" aluminum trays were sprayed level with the Zonollte Mono-Kote material at the Winters Bank site. Spraying and .Curing procedures can he found In Report No. 740301 from our Construction Materials Analysis Deot. (See attached report).
The sampling nozzle I.D. necessary to produce an lso-kinetic sampling condi tion (a condition in which the velocity inside the sampling probe is the same as the air velocity Inside the duct being sampled) was calculated, and two (2) suitable probes fabricated. One sampler probe was installed in the duct approx imately one (1) foot upstream of the two trays of Zonollte Mono-Kote being tested, and approximately one (1) inch higher than the surface of the Zonollte Mono-Kote. The two (2) trays of sample material were installed in cutouts in the floor of the duct such that the surface of the Zonollte Mono-Kote was nearly flush with the floor of the duct. The 6 foot section of duct in .which the samples; were placed was of rectangular cross-section,"12" wide and 6" high (see sketch in Appendix C.)
The sampling rate was held constant by use of fixed orifices which are factorycalibrated to allow a flow of li liters per minute of air providing the pressure on the downstream side is 53Z or 1 ss of the pressure on the upstream side. This pressure drop was monitored bv bourdon tube gages. Air was drawn through the sam pling system by means of a vacuum pump. (See schematic in Appendix C).
The air velocity in the duct was brought up slowly to 50 moh and held there for 10 minutes to purge any loose particles present In the duct or on the Zonollte Mono-Kote. Sampling was then begun at bpth sampling probes and was continued for 24 hours. The sampling filters were changed each eight (8) hours.
The auantltv of dust collected was determined hv veithing. The filter disbs were dried prior to weighing for one (1) hour in sj'C chamber, and *.ept in a dessicator until immediately hefore weighing. After the eight (8) hour sampling period, the filters were dried in the same manner hefore final weighing.
The purpose of the upstream sample is to establish the ambient dust level, which can then he subtracted from the total, leaving onlv the dust contributed bv the Zonollte Mono-Kote.
This establishes an amount of dust per cubic foot of air, which can Ke related to the total amount of airflow through the duct during the test which in turn yeilds the total dust evolved from the Zonollte Mono-Kote surface area.
Duct airflow was established bv means of a velocity profile which can be round on the data sheets in Appendix C.
Lab. Report N'o. 7401 Oh
10037V1<4
BOWSER MORNER
Testing laboratories, Inc.
Vv^i>ER"^/l0R2sfHR ....^Du-tlru^ Jlukroxa.bo'ilLi., fjnc.
CKEMifTS INSPECTORS ENGINEERS Foundti IS! l
. - 4ic Oavis * . i`. .
MAIL A30SE5' = 3. ; ;
0*rroN. in,; j`j
?HCnE 2il-iCi
October 5, 1970
Preczinger and Preczinger Architects and Engineers 1155 Reibold 3uildlng Dayton, Ohio 45402
Attn: Mr. Albert Pretzinger
Re: Lab. Report No. 740301 a'-a*v.jjr-ri-.iWtM-",>.Zonolite Mono-Kota -Testing
Dear Sir:
On July 6, 1970, Zonolite Mono-Kite Material was sampled at the Winterb Bank Project. Three (3) pans and nine (9 cube molds were filled by having the MonoKoce sprayed directly into the molds. The specimens remained on the project sice ovemigr.t in an air-conditioned office and were taken to the Laboratory on July 7, 1970. All specimens were chen room cured at normal temperature for 28+ days. The above sampling and curing nechods had been prearranged at che meeting of July 2, 1970, Sc. Mary's Kail, University of Dayton.
Cn September 15 through 19, 1970, 'vir.c-Tunncl 7:t,.
s were conducted on the
pan samples at Bowser-Morner Testing U_p-ratories. hie.-.--
- to Report No. 740300
of the Product Evaluation Laboratory for detailed ptocecuteo _.
sc results.
On September 25 , 1970, eight (3) cwo inch (2") cubes of Mono-.soce were tested for density and Compressive Strength, after having previously been dried in accordance with A.S.T.M. C472. These cubes represented che same material as that tested for winderosion .
10037937
I
Pretz
and Preczinger
Lad. 1 t. Su. 740301
uc:o' 5, 1970
Page l
Density. PCF
25.2 26.9 25.5 25.9 26.2 27.4 26.5 25.9
26.2 (Average)
-3-?reczinger & Pretzinger 1-ri.le 1-Thomas W. Schommer 1-Div. Ill
TVIS/bla
(c
Compressive Scrcngth, PSI 34.6 43.0 42.5 42.5 40.2 39.0 45.5 43.6 42.0 (Average)
Respectfully submitted. baratorles, Inc.
Thomas W. Schommer Manager, Materials Analysis Laboratory Construction Materials Division
10037939
B0WSER-M0RNER Testing Laboratories, Inc.