Document 37QN00x8OpVXekZJYq7aeyKB3
; Monsanto
. FROM (NAME & LOCATION)
C. D. Bias
DATE February 27, 1968
* SUBJECT
Atwood Adhesives
REFERENCE
WR 68-18
TO K. A. Wells - B-3-N
c*jA. W. M. Coaker - Res 3
S/ J. R. Darby - Res 2
W. F.Waychoff - WWAYC
W. K. Johnson - WJ0HN N. V/. Touchette - Res 3
J. A. Cannon - Res 3
C. Paton - CPAT0 E. C. Wilde - EWILD
i
: ,,
i
; '
We prepared the following adhesives for water immer
sion testing, per Fed. Test Method Std. No. 101a,
Method 116:
.
A BCD
Gelva TS-65
90 90 90 90
Santicizer 885 10
9 99
Santicizer. 8
1
Aroclor 125^
1
Aroclor 5^60
1
...
Two types of paper`were received for testing. One type,
sent to us'by Crown'Zelle^a'ch, was V3c, a corrugated
fiberboard. The other type, sent by the paper group,
was-labeled "Solid Sulfite Board." ^his paper should
have been Type Vis or V2s. When we tried to test the
strength of the adhesive bond on the Instron after
water immersion, all samples of the latter type showed
failure of the paper itself, so that we could not
measure the sheer strength of the adhesive bond. The
corrugated paper samples behaved normally, with the
following results:
.
Sheer Strength, PSI
A 0.96
B 1.02
C 1.23 D 1.11
These results are averages of ten samples each. Sample C, containing Aroclor 125^, was definitely better than the other three. I am somewhat surprised that "B" was only slightly better than "A". I would have thought there would be a greater difference between the two.
If you want these formulations retested, we will have to
have more V3c or V3s from Crown Zellerbach, preferably
about a pound, or at least a dozen sheets one foot square.
We would also need a like amount of Vis or V2s solid
; fiberboard. :
.
STLCOPCB4092287