Caroclohsj.. f-24E-
As Used in Chlorinated Rubber
Monsanto Technical Bulletin No. P-124
January 1, 1948
' Monsanto Chemical Company, St. Louis 4, Mo.
AROCLORS As Usod in C hlorinated Rubber
AROCLORS, chlorinated biphenyl and chlorinated poly-phenyls, are effective plasti cizers and resins for chlorinated rubber base lacquers, varnishes and paints.
These protective coatings are used where ffame resistance, corrosion resistance, chemical resistance, i.e., resistance to adds, alkalies and water, and good electrical insulating properties are required.
Some of the important applications for these protective and decorative coatings for wood, metal, brick, stone, concrete and fabric surfaces include:
i. Wood and metal used in the construction of yachts, barges and other marine craft.
. Structure! steel for bridges, buildings, roofs and power-line structures.
y Structural materials used at chemical plants, pulp and paper mills, textile mills, petroleum refineries and gas works where protection against add fumes, alkalies and gas is essential.
4. For the protection of tank cars and other rolling stock and construction machinery against corrosive materials and w'cathcring.
5. To protect equipment used in electroplating and as stop-off lacquers in this industry.
. Masonry floors and walls. Concrete swimming pools and traffic paints.
7. As cable coatings requiring nonflammability, chemical resistance, water resistance 6nd excellent electrical properties.
8. Coatings for doth to impart "waterproofing" qualities as well as chemical and flame resistance.
*/iROCLOR-I<cg. U.S. Pat. Off.
'
Iho Irvfpnvioiioh (onioln.d In thl, bvllotln i>, * awr bait
j.( trva and advrafa, but all f aamman4#tlan ar
ora <wi without fcwaruntoa, ,lno Iho tanrs.rj on, of a*, era bayand ovf *ntrl. Tha A'.ontanta Chamitat
Canipony
any liability In.urrad In annari*n with tha ura at that# data at raagottlan..
fn>ntn r, r.tih.n;
i.ttcn
l>, i,mtt,t oi o*mrt.onJaiion t# a.a any pradatt In canftici w.th
Hitting yalont* tavaring any malarial ar Ita ata.
>2c
>
TO
o u>
>
o
o o
Cc3 r
o
u
0414208
TOWOLDMONOQ31769
MIXED SOLVENTS
70: JO
97:3 83:17 41:7 :35 :17 30:70 18:59:23 64:36 30:30:40 40:60
30:70 70:30 85:15
Acetone: hexane
Acetone: mineral spirits
Benzene: isopentane
Ccllosolve: ethanol (anhydrous): ethyl acetate: xylene
Ccllosolve: turpentine
Cellosolve: turpentine : mineral spirits
Ethyl acetate: isopentane
Ethyl acetate: isopropyl acetate : Troluoil
Methyl isobutyl ketone: Troluoil
Hi-Flash solvent naphtha : turpentine
Methyl acetate: isopentane
Shell TS-28 : xylene
IV. AROCLOR AND CHLORINATED RUBBER, PLASTICS FILMS
The resinous Arodors 1262 and 5460 show good miscibility with chlorinated rubber films as laid down from toluene solution containing 20 per cent of the plastics, using 2:1 and x: 1, Parlon: resin, ratios. Similarly, the plasticizer type Aroclor 1242, X254 and 1260 show good miscibility in chlori nated rubber. The properties of films derived from the following formulations containing either Parlon and resinous-s. Aroclors 1262 or 5460, or Parlon and the plasticizer type Aroclors 1242,1254 or 1260 were studied.
RESINOUS TYPE AROCLOR FOR PARLON PLASTICS
Ingredients
Pailon, 20-cp......................................
Aroclor 54Co...................................... Dibutyl phthalate..............................
Tung oil, Thermolyzed, 976 .... Xylcuc or butyl acetate................... .... 76
l6 8 4
72
Parts by weight 16 X2 8 12
5 71 76
12 12 3
73
12 12
3-75 72.25
PLASTICIZER TYPE AROCLORS FOR PARLON PLASTICS
Ingredients
Parts by weight
Parlon, 20-cp......................................
20 20
Aroclor 1254 or 1260.......................
7 20
Xylene............................................. .... 76 73 70
Examination of the films cast from these lacquers revealed the following characteristics imparted by
the Aroclors:
Adhesion:--- Unphsticizcd chlorinated rubber films have very poor adhesive qualities. The lacquer film containing Aroclor 5460 gave good adhesion to aluminum, bare steel, primed steel, galvanized iron and Transitc surfaces. Other commercially available resins, particularly oil modified alkyd resins, tested in similar films gave better adhesion than Aroclor 5460 to such suifuecs as glass, tin, copper, scaled wood and cellophane. The lacquer films plasticized with Aroclors 1254 or 1260 gave good adhesion to Transire, cello phane, galvar.i. ed iron and primed steel surfaces. Some of the other commercially available plasticizers tested in similar films gave better adhesion than the Arodors to aluminum, tin, bare sted, copper end scaled wood surfaces. Aroclors, alone, possess pronounced adhesive qualifies. Doubtless, where the objective is to produce adhesives, by varying the Aroclor content or by using a mixture of Arodors in the chlorinated rubber lacquers, much better adhesion to all of the surfaces would be accomplished than was the case with the type of plai.tics films studied. Resistance to Aqueous. Solutions:-- Arodors 1254 or 1260 used as pbstirizers and Aroclor 5460 used as a resin in chlorinated rubber produced plastics films possessing satisfactory resistance to 10 per cent hydrochloric acid, 5 per cent sodium hydroxide, 5 per cent sodium chloride solutions and to v.atcr spot tests.
5--
TOWOLDMONOQ31770
oo
Film Hardness.'-- Using Aroclor 5460 in ratios of 5 : to and 10:10, Aroclor: Parlon, decidedly
softer films were produced than when other commercial resins were similarly used. Likewise,
Aroclors 1254 or 1260 used in ratios of 2:20 and 5:10, Arodor: Parlon, gave softer films
than obtained from other commcrdal plasticizers, used at these concentrations. This indicates
the strong plasticizing action of these Aroclors on chlorinated rubber.
Cold-Check Resistance:-- Regarding cold-check resistant qualities imparted to chlorinated rubber films, Arodor 5460 is somewhat superior to Bakclite type resins, but not as good as long-oil modified alkvds. Arodor 1260 used as a plasticizer rates, in terms of cold-check resist ance, somewhat better than Arodor 1254 and nearly as good as the best of the other plastidzers studied for this property.
Miscellaneous Properties:--Parlon plastics films containing Aroclors 5460, 1254 or 1260 have entirely satisfactory sanding and polishing characteristics.
WeathcrabilityPigmented chlorinated rubber finishes containing Aroclors have consistently Shown good outdoor wcathcrability. However, similar uopigmented finishes, regardless of the plasticizer or resin used and also in the absence of these additives, have been found to give poor outdoor.weathering. Relatively poor resistance to ultraviolet light is a weakness of chlori nated rubber.
Most pigments, with the exception of ultra-marine blue arc usable with Parlon finishes and are recommended when the coating is to be subjected to outdoor weathering or exposed to ultra violet light. However, there is considerable variation regarding the protection offered by different pigments. Inspection of Parlon-fortificd alkyd enamels showed the wcathcrability varied from 63 months for the enamel pigmented with chrome green to 4 months for enamel pigmented with a titanium dioxide-iron blue combination.
V. USES FOR AROCLORS IN CHLORINATED RUBBER COATINGS
A. Finishes for Alkaline Surfaces:
Aroclors, as well as chlorinated rubber, arc highly resistant against alkalies and moisture. Because of these properties paints based on Arodor and chlorinated rubber combinations are used in large quantity for application to concrete floors, walls, swimming pools, etc Examples of this type of paint arc given in Table IV.
TABLE IV. AROCLOR PLASTICIZER IN CHLORINATED RUBBER PAINTS
FOR ALKALINE SURFACES
(Examples of starting formulas)
Materials
Formula x for basement floors
Formula 2 to meet Fed. Spec. TT-P-91
Formula 3 for awimminp pools
(Parts by weight)
Parlon, 20-cp. type..................................
18
18
14.6
Aroclor 1254......................................... .
10
10
4.4
Rczyl 863............................................. ..
8
Aroc'or 5./0 or Cumar P10 ......
6
Rcckosol 31.............................................
2.9
Tung oil, Thermolyzed, 976...................
4.4
Titanium dioxide......................................
16
16
19.7
Zinc oxide.................................................
2
2
6.5
Silica flour.................................................
3
.
Cr:bon black..................................... ... . Xylene................................. ......................
0.2 42.8
0.5 47.5
Hi-r!ash naphtha......................................_________
_________
_____ 47.5
Totals..........................................
100
100 *"*
100
B. Acids and Alkali-Resinlcnt Firrirhcs:
Particular care must be exercised in the choice of resins and plasticizers for use in chemical resistant painis. For this purpose, Aroclors arc outstanding and are being used successfully in the acid and alkali-resistant chlorinated rubber formulations given in 'Fable V.
--6--
OAl'iZIO
TOWOLDMONOQ31771
TABLE VII. RESINS AND PLASTICIZERS MISCIBLE IN PARLON
RESINS
Ambcrol 801, S06P, ST-137, F7
Aroclor 1262, 5460
'
Aroplaz $20, 930, 935,940
Bakcliic XR-3180, XR-4503, XR-4006>
BR-2963, XJ-9S68, BR-1329, BR-3360
Bcckacitc 1112
Bcckar.-.inc r-i^S, P-254
Supcr-Bcckamine 3501
BcckopoJ 1400
Bcckosol 1 (solid), 18, 31, 34,40,1329
Beetle Resin 227-8
Clorafin 70
.
Copal
Cumar Pro
Dammar
Duraplex C-45-LV, C-48, C-49, C-50-LV, C-5X,
C-62, D-61, D-62, E-71, E-71-A, E-73
East India gum
Ester gum
Ethyl Methacrylate
Estcrol 750
Formvar
Gclva 2.5
Glyptal 1247,2450,2454,2458,2464,2466,2500
Lcwisol 2L, 28,33
Methyl Methacrylate Polymers
Neville R-3, R-io
Pcntalyn A, G, M, X
Petrex I, X30H
Phcnac 633-M
Rezyl n6, X315, 412, 775, 803, 807, 829, 869, E8o, X103
Rosin
Santolitc M1IP Staybclitc Ester 1, 2, xo
Staybclitc resin
-
Supcr-Bcckacite 1001
Syntex Hi, H3, H12,17,213,22,28,29,32,36
Tcglac 15, Z-152
Veisicol AD6-3
Vinsol
Amylchloro naphthalene Amyl olcc.ic Amyl stearate Aroclor 1242 Aroclor 1254 Aroclor 1260 Butyl myristate Butyl stearate
Camphor Castor oil, rasv Castor oil, dehydrated Castor oil fatty acid esters Ccllosolvc phthalate Coconut fatty acid esters Diamyl naphthalene
Diamyl phthaiatc Dibutyl phthr.htc
Dibutyl sebacatc Diethyl phtb.alatc Dimethyl pluhalatc Fish oil Hercolyn
Linseed oil
PLASTICIZERS
Methyl ccllosolvc oleate Monoamyl naphthalene Naftolcn * Neville heavy oil No. 2 Ncvillitc oil Oiticica oil Palm fatty acid esters Pcrilla oil Polyamyl naphthalene Resinous Products C-24 Santicizer B-16 Santicizcr M-17 Scxtol phthalatc Scxtol stearate Soya bean fatty acid esters Soya bean oil Thermoil A Tributyl phosphate Tricresyl phosphate Tricthyl citrate Triphcnyl phosphate Tung oil, Thermolyzcd, 97
The strong points and limitations of the resins and plasticizers given in Table VII relative to the progenies they impart to chlorinated rubber are known. None give the important over-all desired qualities attained by the use of Arodors. If occasion arises to consider the use of these materials in specific applications for cldorinated rubber, then more detailed information about them will be given.
i
--9--
041*211
TOWOLDMONOQ31772
The Aroctor compounds impart the following advantages to the films cast from these lacquers:
Adhesion
.
Unplasticized chlorinated-rubber films have very poor adhesion. The lacquer film containing Aroclor 5460 adheres well to aluminum, bare steel, primed steel, galvanized iron, and Transite surfaces. The lacquer films plasticized with Aroclor 1254 or 1260 give good adhesion to Trans-1- ^ ite, cellophane, galvanized iron, and primed-stccl surfaces.
Though compounds with an Aroclor alone possess pronounced adhe sion qualities, better adhesion to all of the surfaces results if mixtures of Aroclor or varied contents are used.
Resistance to Aqueous Solutions
Chlorinated-rubber films with Aroclor 1254 or 1260 (plasticizers) and Aroclor 5460 (resin) show' satisfactory resistance to solutions of 10-per
cent hydrochloric acid, 5-per cent sodium hydroxide, 5-per cent sodium chloride, and water-spot tests.
Film Hardness
Softer films are produced with Aroclor 5460 in ratios of 5:10 and 10:10;
; (Aroclor and Parlon) than with other commercial resins in similar
| mixtures. Likewise, softer films result from Aroclor 1254 or 1260 in
' ratios of 2:10 and 5:10 (Aroclor and Parlon) than with other comj mcrcial plasticizers at these concentrations. These tests show that
Aroclor compounds have strong plasticizing action on chlorinated
rubber.
---
*" Cold-Check Resistance
Aroclor 5460 is superior to phenol-formaldehyde resins in cold-check resistance imparled to chlorinated-rubber films, but not as good as long-oil-alkyd modification. Arocloi; 1260 is a somewhat better plasti cizer than Aroclor 1254.
Weather Resistance
Pigmented chlorinated-rubber finishes containing Aroclor have con sistently withstood outdoor weather tests, but unpigmented finishes do not weather well regardless of the resin or plasticizer used.
Poor resistance to ultraviolet light is also a weakness of chlorinated rubber. Most pigments (except ultramarine blue) are usable with Parlon and are recommended if the coating is to be subjected to outdoor weather or ultraviolet light. However, pigment protection varies con siderably. Inspection of alkyd enamels fortified with Parlon showed weatber.ibility varied from 63 months with chrome green to 4 months for titanium dioxide-iron blue combinations.
Sanding and Polishing Properties
Plastic films compounded with Tarlon and Aroclor 5460, 1254, or 1200 have showed satisfactory sanding and polishing characteristics.