Document 06zBbX8GbDvQ5aQ2RJjpVX52d

AR226-2112 Sample Date Range Concentration Range Action Level Industrial H ygiene 1/1/84 12/31/84 100% Sample Dt Sample# Duration Type Employee Name BTO: 08 TEFLON LOC: 701 FINE POWDER DRYER-EAST SIDE#2 1/8/84 46247 390 Z 1/13/84 46248 380 Z 3/11/84 46249 360 z 4/10/84 46250 395 z 5/7/84 46251 380 z 6/3/84 46252 380 z 7/2/84 46253 360 z 7/30/04 46254 360 z 8/24/84 46255 330 z 9/23/84 46256 420 z 10/21/84 46257 360 z 12/17/84 46258 370 z Pers Chemical C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 Cone Unit Percent 82 MPB 146429%** 0.19 MPB 339% 0,31 MPB 55.4% OZI MPB 379% 0.47 MPB 839% 0.29 MPB 51.8% 0 .0 3 MPB 5.4% 0.26 MPB 509% QJ53 MPB 94.6% 0.62 MPB 110.7%** 056 MPB 64.3% 0.39 MPB 69.6% BTO: 08 TEFLON LOC : 702 FINE POWDER DRYER CONTROL ROOM (ALSO SEE TTF031 1/23/84 3656$ 345 z C-8/FC-143 1/27/84 36587 420 z C-8/FC-143 2/20/84 36568 360 z C-8/FC-143 3/17/84 36569 360 z C-8/FC-143 6/12/84 36570 385 z C-8/FC-143 7/8/84 36571 340 z C-8/PC-143 8/4/84 36572 420 z C-8/FC-143 10/2/84 36573 360 z ' C-8/FC-143 11/2484 36574 350 z C-8/FC-143 12/23/84 36575 340 z C-8/FC-143 0.62 MPB 0.51 MPB 038 MPB 0.37 MPB 0.S3 MPB 0.15 MPB 0.38 MPB 0.77 MPB 0.26 MPB 0.23 MPB <1 110.7%** 91.1% 679% 66.1% 94.6% 26.8% 67,9% 137.5%** 46.4% 41.1% BTO! 08 TEFLON LOC: 704 A/3 - FINE POWDER C-8 WEIGH HOOD 1/8/84 34863 390 z 3/12/84 34864 375 z 7/25/84 34865 360 z C-6/FC-143 C-8/FC-143 C-8/FC-143 . 0.17 MPB 0.15 MPB 0.8 MPB 30.4% 26.8% 142.9%** Tuesday, January 16,2001 10:12:03 AW Page 1 of23 AJP03926 EID 113060 Sample D t S am ple# D uration Type Em ployee Name BTO: 08 TEFLON LOG ; 706 DISPERSION PACKOUT AREA 1/8/84 37365 Z300 7/2384 37356 z360 BTO: OS TEFLON LOG: 70S FINE POWDER DRYER #3 1/13/84 34209 z390 2/20/84 34210 z360 3/11/84 34211 z360 4/19/84 34212 z370 5/7/84 34213 z390 6/3/84 34214 z380 6/12/84 34215 z360 7/30/84 34216 z360 8/5/84 34217 z360 9/26/84 34218 z360 10/2/84 34219 z360 12/23/84 34220 z340 BTO: 0B TEFLON LOG : 70S P/S - FINE POWDER PACKOUT <08PJ) 6/12/84 9392 p380 7/2/84 9393 p360 7/3/84 9394 p345 BTO: 08 TEFLON LOG: 710 FP&D AUTOCLAVE CONTROL ROOM 3/11/84 46024 z360 3/29/84 46025 z390 3/29/84 46026 390 z BTO : 08 TEFLON LOG : 712 NORTH END OF DRYER #3 1Z27/B4 46316 z420 BTO : 08 TEFLON LOC: 713 FINE POWDER OFFICE AREA-GENERAL 6/13/84 46336 375 z Pera Chem ical Cone Unit percent C-8/FC-143 C-8/FC-143 0.04 MPB 0.13 MPB 7.1% 23.2% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 C-S/FC-143 C-S/FC-143 C-S/FC-143 C-8/FC-143 C-S/FC-143 C-S/FC-143 C-8/FC-143 OS MPB 0.93 MPB 0.34 MPB 0.09 MPB 0.48 MPB 0.7 MPB 0.46 MPB 036 MPB 0.54 MPB 0.65 MPB 0.91 MPB 0.25 MPB 89.3% 166.1%" 60,7% 16.1% 85.7% 125.0%** 8Z1% 64.3% 9614% 1131%" 162.5%** 44.6% none none none C-8/FC-143 C-S/FC-143 C-8/FC-143 0.06 MPB 0.06 MPB 0.14 MPB 10.7% 10.7% 25.0% C-S/FC-143 C-S/FC-143 C-S/FC-143 0.06 MPB 0.04 MPB 0.04 MPB 10.7% 7.1% 7.1% C-S/FC-143 0.26 MPB 46.4% C-S/FC-143 0.09 MPB 16.1% Tuesday, January 16,2001 10:12:03 AM .................... ........ -....- - Page 2 of23 AJP003927 EID 113061 Sam ple D t Sam ple # D uration T yp e Em ployee Name BTO: OB TEFLON LOG : 715 SOUTH END DRYER #2 48/84 45081 395 Z 4/20/84 45982 420 z 7/2/84 45383 390 z 8/24/84 45984 330 z 10/21/84 45985 360 z 12/17/84 -986 370 z BTO! 08 LOC: 719 TEFLON MOISTURE CHECK 7/8/84 29559 340 P 7/30/84 29560 360 P 8/1/84 29561 390 p BTO : 08 TEFLON LOC: 726 AISLE IN FRONT OF WAX SEPARATOR 4/29/84 35485 390 z BTO : 08 LOC: 720 TEFLON WAX ROOM- B-162 -1ST FLOOR 1/23/84 37179 345 z 3/17/84 37180 360 z 7/8/84 37181 345 z - 90/84 37182 360 z 11/2464 37183 355 z BTO : 08 LOG: 733 TEFLON TABLDG-DRYER 4/664 39943 360 z 4/664 38944 300 z BTO : 08 LOC: 800 TEFLON P/S-DISPERSION PACKOUT (08PH) 5/764 29435 390 p 5 6 6 4 29436 420 p 6 0 6 4 29437 345 p 6/564 29438 1 p 6/1264 29439 375 p 12/1764 29440 340 p Tuesday, January 16,2001 10:12:03 AM Pera Chem ical Cone U nit Percent C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.03 MPB 0.11 MPB 0.16 MPB 2.03 MPB 0.21 MPB 0.18 MPB 5.4% 19.6% 28.6% 362.5% ** 37,5% 32.1% none none none C-8/FC-143 C-8/FC-143 C-8/FC-143 0.25 MPB <0.03 MPB <0.03 MPB 44.6% 5.4% 5.4% C-8/FC-143 0.08 MPB 14.3% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.23 MPB 0.13 MPB 0,26 MPB 0.65 MPB 0.29 MPB 41.1% 23.2% 46.4% 116.1% 51.8% C-8/FC-143 C-8/FC-143 <0.03 MPB <0.03 MPB 5.4% 5.4% none none none none none none C-8/FC-143 C-8/FC-143 C-8/FC-143 C-6/FC-143 C-8/FC-143 C-8/FC-143 0.08 MPB 0.06 MPB 0.07 MPB 0.09 MPB 0.15 MPB 0.04 MPB 14.3% 10.7% 12.5% 151% 28.8% 7.1% Page 3 of 23 AJP003928 EID 113062 Sam ple D t S am ple# Duration Type Em ployee Name 12/18/B4 29441 12/23184 29442 360 P 3 P Pers Chem ical none C-e/FC-143 none C-8/FC-143 BTO : 08 TEFLON LOG*. 802 PIS - FINE POWDER DRYER OPERATOR (09PI) 1/8/84 29406 390 P 1/13/84 29407 370 P 1/18/34 46090 390 Z 1/23/84 29408 340 P 1/24/84 29409 360 P 1/27/84 29410 420 P 8/24/94 29411 330 P 8/25/54 29412 405 P none C-8/FC-143 none C-8/FC-143 C-8/FC-443 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-e/FC-143 none C-8/FC-143 BTO : 08 TEFLON LOC : 80S P/S- VORTAC MILL PACKOUT 4/7/84 29619 32 P ` none C-8/FC-143 BTO : 08 TEFLON LOC: 804 P/S - FINE POWDER AUTOCLAVE OPERATOR (08PE) 3/5/84 29516 375 P none 3/5/84 29517 375 P none 3/11/84 29518 360 P none 3/17/84 29519 360 P none 3/17/84 29520 360 P none 3/29/84 29521 3O P none 3/29/84 29522 390 P none 9/12/84 29523 180 P none 10/2/84 29524 360 P none 10/21/84 29525 360 P none 10/22/84 29526 330 P none C-8/FC-143 C-e/FC-143 C-8/FC-143 C-6/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 Ce/FC-143 C-e/FC-143 C-8/FC-143 BTO : 08 TEFLON LOC: 805 P/S-FINE POWDER FINISHING DISPERSION OP (0BPH 4/B/B4 29364 410 P none 4/10/84 29365 395 P none 4/19/84 29366 4/20/84 29367 4/29/84 29368 393 P 405 P 390 P none none none 11/24/84 29869 3 P none C-8/FC-143 C-e/FC-143 C-e/FC-143 C-e/FC-143 C-8/FC-143 C-e/FC-143 Tuesday, January 16,2001 10:12:03 AM Cone Unit 0.05 MPB <0.03 MPB Percent 8.9% 5.4% 0.4 MPB 0.06 MPB 0.05 MPB 0.13 MPB 0.07 MPB 0.06 MPB 0.38 MPB 0.3 MPB 71.4% 10.7% 8.9% 23.2% 12.5% 10.7% 67.9% 53.6% 0.15 MPB 26.8% 0,22 MPB 1.29 MPB 0.12 MPB 0.08 MPB 0.06 MPB 0.04 MPB 0.04 MPB 0.51 MPB 0.29 MPB 0.65 MPB 0.16 MPB 39.3% 230.4% 21.4% 14.3% 10.7% 7.1% 7.1% 91,1% 51.8% 116.1% 28.6% 0.04 MPB <0.03 MPB <0.03 MPB 0.04 MPB 0.07 MPB 0.28 MPB 7.1% : 5.4% 5.4% 7.1% 12.5% 50.0% AJP003929 EID 113063 Sample D t S am ple# D uration Type Employee Name Pers Chem ical BTO : 08 TEFLON LOG: 807 P/S - ENVIRONMENTAL CONTROL OPERATOR 2/20184 29456 360 P 9/3/84 29472 360 P 9/23/84 29473 420 P 9/26/84 29474 360 P BTO : 08 TEFLON LOG : 808 PIS-GRANULAR PKOPERATOR (08PF) 4/5/84 29920 360 P 4/6/84 29821 385 P 4/8/84 29622 360 P 4/6/84 29623 538 P BTO : 08 L0C : 861 TEFLON B-163 LAB GENERAL (NOW TCP411) 2/24/84 30764 280 P BTO: 17 RESEARCH LOG: 019 WEIGH AND ADD C-8 TO POLYKETTLE 1/13/84 12116 409 P 8/17/84 12117 380 P BTO: 17 RESEARCH LOG: 066 FLUOROCARBON PANEL BOARD 1/13/84 12224 414 P 6/21/B4 12225 300 P BTO: 17 RESEARCH LOC : 103 P/S FP POLLYKETTLE OPERATOR (17LG) 2/24/84 9132 360 P 6/21/84 9133 367 P 8/17/84 9134 380 P 9/17/84 9135 360 P 9/17/84 9136 360 P 10/16/84 9137 360 P 10/16/84 9138 360 P 11/18/84 14634 361 P 11/18/84 14635 360 P Tuesday, January 16,2001 10:1203 AM none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none 08/F 0143 none C-8/FC-143 none G43/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-B/FC-143 none C-S/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 Cone Unit Percent 0.13 MPB 0.44 MPB 0.06 MPB 0.11 MPB 23.2% 78.6% 10.7% 19.6% 0.04 MPB 0 .0 3 MPB 0.05 MPB 0.03 MPB 7.1% 5.4% 8.9% 5.4% 0.11 MPB 19.6% 0.06 MPB 0.34 MPB 10.7% 60.7% 0.06 MPB <0.03 MPB 10.7% 5.4% 0.13 MPB 036 MPB 0.46 MPB 0.24 MPB 0.47 MPB 0.39 MPB 0.39 MPB >1.0 MPB <0.03 MPB 23.2% 64.3% 82.1% 0% 83.9% 69.6% 69.6% 178.6%** 5.4% P age5of23 AJP0Q393Q EID 113064 Sam ple D t Sam ple # Duration Type Em ployee Name 12/5/84 9139 12/6/84 9140 402 P 403 P BTO : 18 LOC : 001 TEFLON COPOLYMERS FEP OVENS NORTH SIDE 1/31/84 39529 462 Z 3/6/84 39630 412 Z 3/6/84 39531 412 Z 5/7/84 39532 455 Z 6/19/84 39533 462 Z 8/15/84 38534 486 Z 10/19/84 39535 467 Z 12/12/84 39536 468 Z BTO: 18 LOC : 002 TEFLON COPOLYMERS FEP OVENS SOUTH SIDE 1/31/84 39497 466 Z 3/6/84 39498 412 Z 3/6/84 39499 412 Z 5/7/84 39500 455 Z 6/19/84 39501 464 Z 7/5/84 39502 468 Z 8/15/84 39503 483 Z 10/10/84 39504 487 Z 11/21/84 39505 482 Z 12/18/84 39506 477 Z BTO: 18 LOC : 003 TEFLON COPOLYMERS #1 OVEN COOLING TOWER 7/23/84 35666 5 Z 10/23/84 36667 475 Z 12/14/84 35688 400 Z BTO: 18 TEFLON COPOLYMERS LOC: 102 TELOMER A -THIRD LEVEL -DISTILLATION 8/5/84 11321 355 P BTO: 18 LOC : 151 TEFLON COPOLYMERS #2 TORUS DISC DRYER SW CORNER 1/10/84 38488 ... . . 445 Z ................................-- .............................. Tuesday, Januaiy 16,2001 10:12:03 AM Pers Chem ical none C-8/FC-143 none C-8/FC-143 Cone U nit 032 MPB 0.16 MPB Percent 39m 28.6% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 008 MPB 0.03 MPB 0.03 MPB 0.1 MPB 0.23 MPB 0 .0 3 MPB 0.04 MPB 008 MPB 14.3% 5.4% 5,4% 170% 41.1% 5.4% 7.1% 14.3% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.09 MPB 0.44 MPB 0.44 MPB 0.1 MPB 0.28 MPB 0.56 MPB 0 .0 3 MPB 0.13 MPB 0.06 MPB 0.09 MPB 16.1% 78.6% 78.6% 17.9% 50.0% 100.0% * 5.4% 23.2% 10.7% 16.1% C-8/FC-143 C-8/FC-143 C-8/FC-143 0.05 MPB 0.04 MPB 0.16 MPB 8.9% . 7.1% 28.6% none C-8/FC-143 0 .0 3 MPB S.4% C-8/FC-143 ... . ... , r .. , , 0.17 MPB 30.4% P age6of23 AJP003931 EID 113065 Sample D t S am p le# Duration Type Em ployee Name 2/6/84 38489 466 Z 3/8/84 38490 449 Z 4/5/84 38401 2 z 4/5/84 38402 422 z 5/3/84 38493 475 z 6/1/84 38494 458 z 6/14/84 38495 463 z 7/23/84 38406 461 z 8/20/84 38407 467 z 8/28/84 38408 465 z 97I7/B4 38499 10/12/84 38500 11/19/84 38501 12/27/84 38502 480 z 450 z 477 z 500 z BTO : 18 TEFLON COPOLYMERS LOC: 152 #3 & #4 V-DISC PRESS 1/10/84 38374 445 Z 2/6/84 38375 486 z 3/8/84 38376 447 z 4/5/84 38377 423 z 4/5/B4 38378 3 z 5/3/84 38379 476 z 5/30/84 38380 434 z 6/5/84 38381 463 z 6/14/84 38382 465 z 7/11/84 38383 461 z 8/7/84 38384 471 z 8/28/84 38385 467 z 10/16/84 38386 469 z 10/18/84 38387 486 z 11/12/84 38388 483 z 12/10/84 38389 480 z BTO : 18 TEFLON COPOLYMERS LOC: 153 #2 RECYCLE TANK 1/31/84 38630 440 Z 2/14/84 38631 451 Z 3/7/84 38632 441 z ..-- . ....------- . . Tuesday, January 16,2001 10:12:03AM Pere Chem ical C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/F0143 C-8/FC-143 C-8/FC-143 0-84=0143 C-8/FC-143 C-8/FC-143 Cone U nit 0.54 MPB. 0,58 MPB 0.25 MPB 0.25 MPB 0.12 MPB 0.13 MPB 0J34 MPB 0.24 MPB 0.07 MPB 0.25 MPB 0.38 MPB 0.24 MPB 0.37 MPB 0.43 MPB Percent 96.4% 103.6%' 446% 44.6% 21.4% 23.2% 60.7% 42.9% 12.5% 46.4% 67.9% 429% 66.1% 76.8% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.54 MPB 0.61 MPB 0.87 MPB 0.47 MPB 0.47 MPB 0.18 MPB 0.1 MPB 0.43 MPB 0.38 MPB 0.6 MPB 0.45 MPB 0.E3 MPB 0.28 MPB 0.71 MPB 1.60 MPB 0.78 MPB 96.4% 108.9% ** 119.6%** 839% 839% 32.1% 179% 76.8% 679% 107.1%** 80.4% 112.5%** 50.0% 126.8% ** 301.8%** 139.3% ** C-8/FC-143 0.32 MPB C-8/FC-143 0.45 MPB C-8/FC-143 0.56 MPB ... . ......... . .. ...... 57.1% 80.4% 100.0% Page 7 o f23 AJP003932 EID 113066 Sample D t S am ple# Duration Type Employee Name 4/24/84 38633 4/24/84 38634 7/26/84 38635 8/6/84 36638 9/14/84 38637 10/16/84 38538 10/25/84 38839 11/13/84 38640 482 Z 462 Z 466 Z 466 Z 475 Z 4 Z 470 Z 481 Z BTO : 18 TEFLON COPOLYMERS LOC : 154 m FLUFF BOOSTER PUMP 2/14/84 3B990 452 Z 8/9/84 38991 477 Z 9/13/84 38992 466 Z BTO : 18 TEFLON COPOLYMERS LOC! 155 FLOTATION TANK 1/13/84 38326 456 Z 3/20/84 38327 456 Z 4/18/84 38328 432 Z 4/18/84 38329 432 Z 5/4/84 38330 470 Z 6/1/84 38331 461 Z 6/8/84 38332 463 Z 7/12/84 38333 479 Z 7/23/84 38334 461 Z 8/7/84 38335 471 Z 8/20/84 38336 468 Z 9/5/84 38337 465 Z 9/17/84 38338 477 Z 10/5/84 38339 470 Z 10/18/84 38340 484 Z 11/5/84 38341 468 Z 12/27/84 38342 497 Z BTO: 18 TEFLON COPOLYMERS LOC: 156 #2 BAGHOUSE PLATFORM 6/14/84 39135 461 7 7/31/84 39136 45D 2 Tuesday, January 16,2001 10:12:03 AM Pere Chemical C-8/FC-143 C-8/FC-143 C-6/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 Cone U nit 0.2 MPB 0.2 MPB 0.31 MPB 0.31 MPB 0.5 MPB 0.15 MPB 0.15 MPB 0.27 MPB Percent 35.7% 35.7% 55.4% 55.4% 89.3% 268% 26.8% 487% C4S/FC-143 C-8/FC-143 C-8/FC-143 0.53 MPB 0.33 MPB 0.62 MPB 94.6% 58.9% 110.7% " C-8/PC-143 C-8/FC-143 C8/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 C-B/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/F0143 C-8/FC-143 C-8/FC-143 0.95 MPB 1.02 MPB 0.26 MPB 0.26 MPB 0.31 MPB 0.32 MPB 0.6 MPB 0.67 MPB 2.06 MPB 0.45 MPB 0.25 MPB 0.45 MPB 0.87 MPB 1.05 MPB 0.83 MPB 0.15 MPB 034 MPB 169.6% ** 182.1%" 46.4% 46.4% 55.4% 57.1% 107,1%** 119.6% " 367.9% " 80.4% 44.6% 80.4% 155.4% " 187.5% " 148.2% " 26,8% 60.7% C-8/FC-143 C-8/FC-143 . . . . . . . . . 7, . 7 - 0.25 MPB 0.13 MPB .. ..... 44.6% 23.2% . . ... Page 8 of 23 AJP003933 EID 113067 Sam ple Dt S am ple# Duration Type Em ployee Name BTQ : 18 TEFLON COPOLYMERS LOG: 158 FLAKE PACKOUT BIN-BOTTOM 1/16/84 39029 443 Z 2/8/84 39030 457 Z 3/7/84 38031 444 2 4/9/B4 38032 444 Z 4/9/84 38083 444 z 6/15/84 38034 464 z 7/26/84 3903S 469 z 7/30/84 30036 474 z 8/7/84 39037 472 z 8/22/84 39038 469 z 10/15/34 38039 467 z 10/23/84 39040 482 z 11/19/84 38041 477 z 12/13/84 38042 480 z STO: 18 TEFLON COPOLYMERS LOG: 159 #2 SCREW CONVEYOR 1/18/84 39163 4 Z. 2/2/84 39164 459 Z 3/6/84 39165 412 Z 3/8/84 39166 4/3/84 39167 412 Z 429 Z 4/3/84 39168 429 z 5/30/84 39169 455 Z 6/1/84 3917D 457 z 6/1/84 39171 459 z 6/13/84 39172 471 z 7/6/84 39173 472 z 7/23/84 39174 8/3/84 39175 461 z 465 z 8/20/84 39176 467 z 9/11/84 39177 470 z 10/8/84 39178 470 z 10/23/84 39179 484 z 11/12/84 39180 474 z 12/11/84 39181 470 z Tuesday, January 16,2001 10:12:03 AM Pere Chem ical Cone Unit Percent C-a/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.49 MPB 037 MPB 0.34 MPB 0.14 MPB 0.14 MPB 0.43 MPB 038 MPB 0.36 MPB 0.42 MPB 0.62 MPB 0.6 MPB 0.03 MPB 0.38 MPB 0.74 MPB 873% 66.1% 60.7% 230% 25.0% 76.8% 67.9% 64.3% 75.0% 110.7% 142.9% 5.4% 67.9% 132.1% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC4 43 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.59 MPB 0.34 MPB 0.06 MPB 0.06 MPB 0.13 MPB 0.13 MPB 0.1 MPB 0.18 MPB 0.12 MPB 0.65 MPB 1.14 MPB 0.42 MPB 0.39 MPB 0.15 MPB 0.71 MPB 0.51 MPB 0.26 MPB 0.33 MPB 0.81 MPB 105.4%** 60.7% 10.7% 10.7% 23.2% 23.2% 17.9% 32.1% 21.4% 110.1%** 203.6% ** 75.0% 69.6% 26.6% 126.8% ** 91.1% 46.4% 58.9% 144.6%" Page 9 of 23 AJP003934 EID 113068 Sample Dt S am ple# Duration Type Em ployee Name BTO : 18 TEFLON COPOLYMERS LOC: 160 #2 FLAKE HOPPER 1/18B4 38432 445 Z 3/27/S4 38433 4 Z 3/27/84 38434 4 Z 4/18/84 38435 4 Z 4/18/84 38438 4 Z 501/84 38437 465 Z 6/7/84 38438 459 Z 6/13/84 38439 467 Z 6/22/84 38440 458 Z 7/1204 38441 479 Z 8/904 384! 477 Z 9/11/84 3 8 4 470 Z 10/904 38444 479 Z 11/2904 38445 479 Z 12/1304 38446 1 Z BTO : 18 LOC ! 162 TEFLON COPOLYMERS GLOVE BOX 1/2404 38676 480 Z 30/84 38677 456 Z 4/904 38678 444 Z 4/904 38679 444 Z 4/1804 38680 4 Z 4/1804 38681 4 Z 1204 38682 466 Z 7/1204 38683 479 Z 9/504 38684 465 Z BTO: 18 TEFLON COPOLYMERS LOC : 163 #2 MAKE UP AIR SUPPLY 1/3/84 38537 430 Z 1/13/84 38538 7 Z 2/13/84 38539 460 z 3/20/84 38540 456 z 4/30/84 38541 1 z 4/30/84 38542 1 z 5/4/84 3 8 5 470 z 5/22/84 38544 474 z Tuesday, January 16,2001 10:12:03 AM Pera Chem ical Cone Unit Percent C-8/FC-143 C-8/FC-1 C -8 /F C -1 C-8/FG-143 C-8/FC-143 C-8/FC-1 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-1 C-8/FC-143 C-8/FC-1 C-8/FC-143 C-8/FC-143 0 . MPB 0.26 MPB 026 MPB 0.52 MPB Oj52 MPB 0.1 MPB 026 MPB 02 MPB 02 MPB 0.66 MPB 0.27 MPB 0.7 MPB 056 MPB 0.27 MPB 1.04 MPB 82.1% 46.4% 46.4% 929% 92.9% 17.9% 46.4% 35.7% 35.7% 117.9%' .2 % 125.0%' 100.0% 48.2% 185.7% C-8/FC-1 C-8/FC-143 C-8/FC-1 C-8/FC-1 C-8/FC-143 C-0/FC-1 C-8/FC-143 C-8/FC-1 C-6/FC-1 02 MPB 0.13 MPB 0.13 MPB 0.13 MPB 0.18 MPB 0.18 MPB 0.17 MPB 0.68 MPB 0.13 MPB 36.7% 23.2% 232% 23.2% 32.1% 32.1% 30.4% 121.4% 23.2% C-8/FC-1 C-8/FC-1 C-8/FC-1 C-8/FC-1 C-8/FC-143 C-8/FG-1 C-8/FC-1 C-8/FC-1 0.08 MPB 0.72 MPB 0.04 MPB 034 MPB <0.03 MPB <0.03 MPB 0.03 MPB 0.05 MPB 14.3% 128.6% 7.1% '60.7% 5.4% 6.4% 5.4% 8.9% Page 10 of 23 AJP003935 EID 113069 SampleDt sample# Duration Type Employee Name 6/14184 38645 6/21/84 38546 7/16/84 38547 7/26/84 38548 8/14/B4 38549 9/18/84 38550 10/15/84 38561 11/1/84 38652 11/14/84 38553 12/19/84 38554 465 Z 467 Z 361 z 465 z 487 z 432 2 466 Z 465 z 495 2 477 2 BTO : 18 TEFLON COPOLYMERS LOC: 164 B163-60FTROOF 1/3/84 39096 430 2 1/24/84 39097 449 2 2/13/84 38098 460 Z 3/19/84 39099 445 2 4/30/84 39100 451 2 4/30/84 39101 451 Z 5/31/84 39102 466 2 6/14/84 39103 461 Z 7/10/84 39104 477 Z 7/27/84 39105 465 Z 8/14/84 39106 486 Z 8/28/84 39107 467 2 9/14/84 39108 477 Z 10/9/B4 39109 477 z 10/26/34 39110 481 2 11/14/84 39111 495 2 12/19/84 39112 477 2 . BT: 18 TEFLON COPOLYMERS LOC: 165 INITIATOR 1 SUPPLYTANK 1/5/84 39555 432 2 2/B/84 39566 488 2 3/21/84 39557 443 2 4/5/84 39558 422 Z 4/5/84 396 422 Z 5/31/84 39560 467 Z . _ ....... * -l7. _ _ Tuesday, January 16,200110:12:03 AM Pets Chemical C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C8/FC-143 C-8/FC-143 C-3/FC-143 C-8/FC-143 C-8/FG-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C3/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC4 43 Gone Unit 056 MPB 0 .0 3 MPB 0.6 MPB 0,9 MPB 0.12 MPB 0.44 MPB 0.95 MPB 0.09 MPB 0.11 MPB 0.13 MPB Percent 46.4% 5.4% 107.1%** 160.7% " 21.4% 78.6% 98.2% 16.1% 19.6% 23.2% 0.06 MPB 0.04 MPB 0.05 MPB 0.36 MPB 0,06 MPB 0.06 MPB 0.1 MPB 0.27 MPB 0.63 MPB 0.05 MPB 0.1 MPB 0.08 MPB 0.5 MPB 0.29 MPB <0.03 MPB 0.04 MPB 0.08 MPB 10.7% 7.1% 89% 64.3% 10.7% 10.7% 179% 48.2% 1129% " 8.9% 179% 14.3% 893% 51.8% 5.4% 7.1% 143% 0.68 MPB 1.44 MPB 0.29 MPB 0.88 MPB 0.88 MPB 0.35 MPB 121.4% " 257.1%" 513% 157.1%" 157.1% " 62,6% AJP003936 EID 113070 Sample U Sample# Duration Type Employee Nane m m 39661 7/23/84 39562 8/21/84 39563 105/04 39564 10/17/84 39605 12/17/84 39566 462 2 455 Z 466 z 470 z 471 z 474 z BTO: 18 TEFLON COPOLYMERS LOG: 166 FEP DISPERSION AREA SCALE 1/19/84 38947 460 z 3/2/84 38948 445 3/2/84 38949 445 z 4/17/84 36950 469 z 4/17/84 38951 9 z 4/26/84 38952 460 z 4/26/84 38963 6/6/84 38954 460 z 463 z 6/7/84 38955 460 z 6/18/84 38956 482 z 7/10/84 38957 9 z 8/6/84 38958 466 z 9/6/84 38959 469 z 10/11/84 38960 476 z 11/13/84 38961 12/5/84 38962 481 z 477 z BTO: 18 TEFLON COPOLYMERS LOC: 167 FEP DISPERSION STABILIZATION TANKS 1/16/84 38840 4SO z 2/28/84 36841 459 z 2/28/84 38842 459 z 3/22/84 38843 -3 z 4/17/84 38844 459 z 4/17/84 38845 45S z 4/26/84 38846 456 z 4/26/84 38847 . 456 z 6/6/84 38848 466 z 6/7/84 38849 462 z 7/10/84 38850 458 z wwiert---............. *" Tuesday, January 16,2001 10:12:03 AM Pere Chemical C-8/FC-143 C-a/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C3/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 OS/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 08/FC-143 08/FC-143 Cone Unit 1.63 MPB 4.81 MPB 2.64 MPB 0.84 MPB 0.79 MPB 0.47 MPB Percent 291.1%** 868.9%** 471.4%** 150.0%** 141.1%** 83/9% 0.08 MPB 0.08 MPB O.OB MPB 0.15 MPB 0.15 MPB 0.09 MPB 0.09 MPB 0.14 MPB 0.2 MPB 026 MPB 069 MPB 0.08 MPB 025 MPB 0.08 MPB 0.07 MPB 0.14 MPB 143% 143% 143% 263% 263% 16.1% 16.1% 25.0% 35.7% 46.4% 1589%** 14.3% 44.6% 143% 12.5% 25.0% 0.1 MPB 0.12 MPB 0.12 MPB 0.08 MPB 0.1 MPB 0.1 MPB 0.09 MPB 0.09 MPB 0.14 MPB 0.19 MPB 0.63 MPB 179% 21.4% 21.4% 143% 179% 179% 16.1% 16.1% 25.0% 339% 1125%** Page12of23 AJP003937 EID 113071 Sample Dt sample# 8/3/34 38851 9/6/84 38852 10/5/84 38863 11/5/84 38854 12/5(84 38855 Duration Type Employee Name 2468 z461 z470 z407 z469 Pere Chemical C-8/PC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 BTO: 18 TEFLON COPOLYMERS LOCs 168 FEP DISPERSION ADDITION AREA PLATFORM 1/11/84 38789 z444 2/29/84 38790 3 z 2/29/84 38rai z453 3/22/84 38792 z446 4/17/84 38793 z458 4/17/84 38794 z458 4/26/84 38795 z460 4/26/84 38796 z460 6/7/84 38797 z460 6/18/84 38798 z465 7/2Q/B4 38799 z484 8/6/84 38600 z467 9/6/84 38801 z471 11/13/84 38802 z481 12/5/84 38803 z478 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 C-S/FC-143 C-S/FC-143 C-a/FC-143 BTO: 18 TEFLON COPOLYMERS LOC: 169 FEP DISPERSION C-8 RECIRCULATION PUMP 1/12/84 38889 z449 2/29/84 38890 z453 2/29/84 38891 z453 3/22/34 38892 z450 4/17/84 38893 z457 4/17/84 38894 z457 4/26/84 38895 z456 4/26/84 38896 z456 6/6/84 38897 z462 6/18/84 38898 z485 7/20/84 38890 z485 8/8/84 38900 z467 9/7/84 38901 2458 C-8/FC-143 C-a/FC-143 C-S/FC-143 C-S/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-S/FC-143 C-S/FC-143 C-S/FC-143 Tuesday, January 16,2001 10:12:03 AM Cone Unit 0.11 MPB 0.24 MPB 0.08 MPB <0.03 MPB 0.08 MPB Percent 19.6% .9 % 143% 5.4% 14.3% 0.6 MPB 0.0B MPB 0.08 MPB 0.1 MPB 0.11 MPB 0.11 MPB 0.08 MPB 0.08 MPB 0.12 MPB 0.28 MPB 0.44 MPB 0.18 MPB 0.28 MPB 0.08 MPB 0,08 MPB 107.1%** 14.3% 14.3% 17.9% 19.6% 19.6% 14.3% 143% 21.4% 50.0% 78.6% 32.1% 30.0% 14.3% 14.3% 0.16 MPB 0.2 MPB 0 2 MPB 0.21 MPB 0.05 MPB 0.05 MPB 0.09 MPB 0.09 MPB 0.12 MPB 0.24 MPB 0.44 MPB 0.39 MPB 0.23 MPB 28.8% 35.7% 35.7% 37.5% 8.9% 83% 16,1% 16.1% 21.4% 42.9% 78.6% 69.6% 41.1% Page 13 of23 AJP003938 EID 113072 Sample D t S am ple# D uration Type Employee Name 10/11/84 38912 11/6/84 38913 12/6/84 38914 475 Z 472 Z 469 Z BTO: 18 TEFLON COPOLYMERS LOC: 188 B-163 45 FT ROOF 7/2/84 39602 46S Z BTO: 18 TEFLON COPOLYMERS LOC: 189 B-163 MID ROOF H&VINLET 1/3/84 37965 446 Z 2/14/84 37966 493 Z 3/27/84 37967 447 Z 3/27/84 37968 447 2 BTO: 18 TEFLON COPOLYMERS LOC: 202 FEP-POLYKETTLE#1 LOWER CELL 11/7/84 39659 487 Z BTO: 18 LOC: 208 TEFLON COPOLYMERS FEP-BLENDERPIT 1/3/84 34014 447 Z 1/19/84 34015 449 Z 3/9/84 34016 452 Z 4/18/84 34017 445 Z 4/18/84 34018 445 Z 5/31/84 34022 466 Z 6/8/84 34023 465 Z 7/10/84 34024 463 Z 8/9/84 34025 477 Z 9/10/84 34026 466 2 10/8/84 34027 470 Z 10/29/84 34028 <87 2 11/5/84 34029 468 Z 12/10/84 34030 482 Z BTO: 18 TEFLON COPOLYMERS LOC : 210 #1 COAOULATOR-2ND FLOOR 2/8/B4 37244 455 Z 4/30/84 37245 460 Z Tuesday, January 16,2001 10:12:03 AM pers Chemical C-8/FC-143 C-8/FC-143 C-8/FC-143 Cone U n it 0.13 MPB <0.03 MPB <0.03 MPB Percent 23.2% &4% 5.4% C-8/FC-143 <0.03 MPB 5,4% C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.04 MPB 0.04 MPB 0.03 MPB 0.03 MPB 7.1% 7,1% 5.4% 5.4% C-8/FC-143 0.06 MPB 10.7% C-8/FC-143 . C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0.39 MPB 0.42 MPB 0.34 MPB 0.33 MPB 0.33 MPB 0,26 MPB 0.21 MPB 0.67 MPB 0.22 MPB 0.84 MPB 0.46 MPB 037 MPB 0.26 MPB 0.29 MPB 69.6% 75.0% 60.7% 583% 583% 46.4% 37.5% 119.6%** 39.3% 150.0%** 82.1% 66.1% 46.4% 513% C8/FC-143 C-8/FC-143 1.76 MPB 0.83 MPB 3143% ** 148.2% ** Page 14of23 AJP003939 EID 113073 Sample D t S am ple# D uration Type Employee Name Pero Chem ical 430/84 37246 5/22/84 37247 6/5/84 37248 7/23/84 372 8/2/84 37250 10/1/84 37251 10/19/84 37252 11/2/84 37253 12/11/84 37254 12/17/84 37255 460 Z 466 Z 463 Z 456 Z 465 Z 474 Z 482 Z 515 Z 470 Z 481 Z C-8/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 - C-S/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/PC-143 C-a/FC-143 Cone Unit 0.83 MPB 0.77 MPB 0.19 MPB 3.92 MPB 3.64 MPB 0.45 MPB 1.31 MPB 0.56 MPB 3.86 MPB 2,43 MPB Percent 1482% ** 137.5%** 33.9% 700.0%** 650.0%** >.4% 233.9%** 100.0%** 689.3%** 433.9% ** BTO: 18 TEFLON COPOLYMERS LOG: 212 #1 CQA6ULATOR-1ST FLOOR PLATFORM 1/6/84 35561 4<*2 Z 2/8/84 35562 458 Z 3/20(84 35563 456 Z 3/27/84 35564 449 Z 3/27/84 35565 4 Z 4/9/84 35566 4 Z 4/9/84 35567 445 Z 5/3/84 35568 474 Z . 5/22/84 36569 468 Z 6/5/84 35670 461 Z 7/2/84 35671 462 Z 7/23/84 35572 455 Z 8/2/84 35573 466 2 8/21/84 35574 469 Z 9/7/84 35676 457 Z 9/14/84 35576 475 2 10/1/84 35577 476 Z 10/17/B4 35578 483 Z 11/2/84 35579 465 2 12/10/84 355B0 481 Z C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 OS/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-a/FC-143 C-8/FC-143 0.28 MPB 0.1 MPB 0.12 MPB 0.4 MPB 0.4 MPB 0.37 MPB 0.37 MPB 0.13 MPB 0.07 MPB 0.58 MPB 0.08 MPB 0.17 MPB 029 MPB 0.15 MPB 0.26 MPB 0.37 MPB 0.1 MPB 0.06 MPB 3.56 MPB 0.13 MPB 50.0% 17.9% 21.4% 71.4% 71.4% 66.1% 66.1% 232% 12.5% 103.6%** 14.3% 30.4% 51.8% 26.8% 46.4% 661% 17.9% 10.7% 635.7%** 23.2% BTO: 18 TEFLON COPOLYMERS LOG: 214 FEP4I1 TORUS DISK DRYER (CLEAN) ROOM 1/11/84 34937 4 2 2/6/84 34938 465 Z 3/7/84 34909 444 2 ___ ___ _____ __........... ............ .............__..... Tuesday, January 16,2001 10:12:03 AM C-8/FC-143 0.19 MPB C-8/FC-143 0.43 MPB C-8/FC-143 0.85 MPB _. ... . 33.9% 768% 151.8%*' Page 15 of 23 AJP003940 EID 113074 Sample D t S am ple# Duration Type Em ployee Name 4/4/84 34340 4/4/84 34941 5/5784 349 5/11/84 34943 5/22/34 34044 6/11/84 34045 7/5/84 34046 6/6/84 34047 8/16/84 34948 10/22/84 34949 10/24/84 34950 12/17/84 34051 426 Z 426 Z 456 Z 461 Z 465 Z 468 Z 488 Z z466 z477 z474 z477 z476 BTO: 18 TEFLON COPOLYMERS LOG: 215 FEP-POLYKETTLE CONTROL ROOM 2/22/84 35733 441 Z 7/27/84 35734 458 Z BTO: 18 TEFLON COPOLYMERS LOC: 218 P/S-WETFINOP(18PA)ALSOSEETCP149 1/25/B4 10464 455 P 3/21/84 10465 440 P 3/21/84 10466 440 P 6/21/84 10467 434 P 9/12/84 10468 475 P 10/9/84 10469 469 P BTO; 18 TEFLON COPOLYMERS - LOC: 217 FEP CONTROL ROOM-COMPUTER AREA 2/8/84 38265 454 Z BTO : 18 TEFLON COPOLYMERS LOC: 218 FEP FOREMANS OFFICE 11/16/84 39314 484 z BTO: 18 TEFLON COPOLYMERS LOC: 220 #2 COAGULATOR-1ST FLOOR PLATFORM 1/6/84 35838 441 z 2/2/84 35839 456 z 3/2/84 35840 445 z Tuesday, January 16,2001 l a i 2:03 AM Pers Chem ical C-8/FC-143 C-8/FC-143 C-6/FC-143 C-B/FC-143 C-S/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 OS/FC-143 C-S/FC-143 C-S/FC-143 C-S/FC-143 c-e/Fc-143 C-8/FC-143 none C-8/FC-143 none C-S/FC-143 none C-S/FC-143 none C-S/FC-143 none C-8/FC-143 none C-S/FC-143 C-S/FC-143 C-S/FC-143 C-8/FC-143 C-S/FC-143 C-S/FC-143 Cone U nit 0.52 MPB 0.52 MPB 0.48 MPB 0 . MPB 0.5 MPB 0.4 MPB 0.76 MPB 0.41 MPB 0.15 MPB 0.27 MPB 0.16 MPB 0.4 MPB Percent 92.9% 92.9% 65.7% 85.7% 89.3% 71.4% 135.7% 73.2% 266% 48.2% 28.6% 71.4% 0.06 MPB <0.03 MPB 10.7% 5.4% 0.17 MPB <0.03 MPB <0.03 MPB <0.03 MPB 0.16 MPB 0.13 MPB 30.4% 5.4% 5.4% 5.4% 28.6% 232% 0.07 MPB 12.5% 0.05 MPB 8/9% 0.06 MPB 0.24 MPB 0.21 MPB 10.7% 42.9% 37.5% Page 16 of 23 EID 113075 Sam ple D t S am ple# D uration Type Employee Name 3/2/84 35841 4/4/84 35842 4/4/84 35843 5/2/84 35844 5/4/84 35045 6/11/84 35846 6/13/84 36847 8/8/84 38848 8/27/84 36849 0/7/84 35850 10/12/84 35851 11/6/84 35852 12/13/84 358S3 12/18/84 35854 445 2 422 Z Z 467 z 470 z 465 z 463 z 471 z 470 z 456 z 463 z 472 z 481 z 476 z BTOt 18 LOC; 221 TEFLON COPOLYMERS P/S- FEP PROCESS PK OPERATOR (18PA) 1/25/84 11033 461 p '"'3/8/34 f1034 446 p 5/31/84 11035 468 p 6/21/84 11036 432 p 7/27/84 11037 458 p 8/14/84 36071 354 z 8/22/84 11038 465 p 10/26/84 11030 471 p 12/28/84 11040 460 p BTO: 18 LOG: 222 TEFLON COPOLYMERS FEP POLYKETTLE CELL #2 6/21/B4 39608 470 z 9/4/84 39609 @40 z BTO: 18 TEFLON COPOLYMERS LOC: 223 FEP POLYKETTLE CELL #1 2/2/84 39646 465 z 11/2/84 39647 499 z 11/7/84 39648 487 z Pern Chem ical C-S/FC-143 OB/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-S/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-6/FC-143 none C-S/FC-143 C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 C-8/FC-143 C-8/FC-143 C-6/FC-143 C-8/FC-143 C-8/FC-143 Cone U nit 0.21 MPB 029 MPB 029 MPB 0.14 MPB 0.1 MPB 021 MPB 0,11 MPB 0.14 MPB 026 MPB 0.26 MPB 0.63 MPB 0.07 MPB 0.22 MPB 021 MPB Percent 375% 515% 51.8% 25.0% 175% 375% 195% 25.0% .4 % 46.4% 94.6% 125% 39.3% 37.5% .. 0.17 MPB .5 MPB 0 .0 3 MPB 0.9 MPB 0 .0 3 MPB 0.17 MPB 021 MPB 0.09 MPB 0 .0 3 MPB 30.4% 0.9% 5.4% 160.7%** 5.4% 30.4% 37.5% 16.1% 5.4% 0.14 MPB 023 MPB 25.0% 41.1% 0.04 MPB 0.05 MPB 0.09 MPB 7.1% 8.9% 16.1% Tuesday, January 16,2001 10:12:03 AM Page 17 of 23 AJP003942 EID 113076 sam ple D t S am p le# D uration T yp e em ployee Name BT*. 18 TEFLON COPOLYMERS LOC: 225 C-8 PREPARATION AREA 1/5/84 39324 2/1484 39325 2/22/84 39326 3/9/84 39327 4/30/84 30628 4/30/84 30329 5/30/84 30330 434 Z z447 z438 z453 z440 z448 z460 6/12/84 38331 7/20/84 30332 6/10/84 39333 8/21/84 38334 9/10/84 39335 10/8/84 39336 12/4/84 39337 466 z z483 z477 z466 z468 z472 z465 BTO: 18 TEFLON COPOLYMERS LOC: 226 TRAY CONVEYER-OVEN FEED 2/28/84 35407 460 z 2/28/84 35408 0 Z 7/30/84 35409 462 Z 8/13/84 35410 484 Z BTO : 18 TEFLON COPOLYMERS LOC: 227 FEP FLAKE HOPPER 1/12/84 37629 442 Z 2/2/84 37630 3/2/84 37631 3/2/84 37632 457 Z z444 z 4/4/84 37633 423 z 4/4/64 37634 S/1/84 37635 5/1/84 37636 423 z 460 z z460 5/11/84 37637 461 z 5/22/84 37638 6/11/84 37639 465 z z465 6/13/84 37640 7/10/84 37641 462 z z467 8/10/84 37642 478 z Tuesday, January 16, 2001 10:12:03AM Pcrs Chem ical C one U nit Percent C-8/FC-143 C-8/FC-143 C-8/FC-143 C-6/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 2.05 MPB 0.63 MPB 0.05 MPB 0.67 MPB 1.65 MPB 1.65 MPB 0.2 MPB 0.38 MPB 0/91 MPB 0.75 MPB 0.38 MPB 0.34 MPB 0.35 MPB 0.72 MPB 366.1%** 112.5%** 88% 119.6%** 294.6% " 294.6%" 35.7% 67/9% 162.5%** 1339% " 679% 60.7% 62.5% 128.6% " C-8/FC-143 C-8/FG-143 C-e/FC-143 C-8/FC-143 0.18 MPB 0.18 MPB 0.41 MPB 0.05 MPB 321% 32.1% 73.2% 89% C-8/FC-143 OS/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/F-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 1.41 MPB 056 MPB 0.65 MPB 0.65 MPB 0.43 MPB 0.43 MPB 0.14 MPB 0.08 MPB 0.1 MPB 0.13 MPB 039 MPB 0.39 MPB 0.78 MPB 0.49 MPB 251.8% 100.0% 116.1% 116.1% . 76.6% 76.8% 259% 14.3% 17.9% 23.2% 69.6% 69.6% 139.3% 87.5% P a g e l8 o f2 3 EID 113077 Sample D t S am ple# Duration Type Employee Name 10/22/84 37643 10/24/84 37644 11/1/84 37645 12/17/84 37648 474 Z S II z 463 z 471 z BTO: 18 TEFLON COPOLYMERS LOC: 229 P/S - FEP OVEN OPERATOR(18PB) 4/26/84 10999 462 p 10/11/B4 11000 465 p BTO: 18 TEFLON COPOLYMERS LOC: 230 FEP-TRAYOUT 6/8/84 37060 462 Z 7/16/84 37061 360 Z 12/14/84 37D62 478 Z BTO: 10 LOC : 231 TEFLON COPOLYMERS FP-OV6N OR (VACATED 9/97) 12/12/84 37566 467 Z BTO: 18 TEFLON COPOLYMERS LOC: 237 FEP SLAB RACKS (whenslabs present) 2/28/84 36655 457 z 2/28/84 36656 457 z 3/21/84 366S7 442 z 10/18/84 36658 479 z 10/26/84 36659 476 z 11/30/84 36660 475 z 12/14/84 36661 475 z BTO: 18 TEFLON COPOLYMERS LOC: 238 FEP-N01 OVEN PLATFORM 2/7/84 39419 449 Z 7/31/84 39464 445 z BTO : 18 TEFLON COPOLYMERS LOC: 239 FEP-NO 2 OVEN PLATFORM 2/7184 39588 450 Z 7/31/84 39587 445 2 Tuesday, January 16,2001 10:12:03 AM Pers Chem ical C-B/FC-143 08/FC-143 C-8/FG-143 C-8/FC-143 C one U nit 0.19 MPB 0.29 MPB 0.55 MPB 0.99 MPB Percent 33.9% 51.8% 98.2% 1768% none C-8/FC-143 none C-8/FC-143 0 .0 3 MPB 0.11 MPB 5,4% 19.6% C-8/FC-143 C-8/FC-143 C-B/FC-143 0,23 MPB 0.69 MPB 0.53 MPB 41,1% 1235% 94.6% C-8/FC-143 0.07 MPB 128% C-8/FC-143 C-B/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 C-8/FC-143 C-B/FC-143 0.08 MPB 0,08 MPB 0.03 MPB 0.11 MPB 0.12 MPB <0.03 MPB 0.12 MPB 14.3% 14.3% 5,4% 19.6% 21.4% 5.4% 21.4% C-8/FC-143 C8/FC-143 0.03 MPB 0.16 MPB 5.4% 28.6% C-8/FC-143 C-8/FC-143 0.13 MPB 0.11 MPB 23.2% 19.6% Page 19 of 23 AJP003943 EID 113078 Sample D t S am ple# Duration T yp e Employee Name STO: 18 TEFLON COPOLYMERS LOG: 244 FEP SLAB STRIPPER 3/19/84 37319 443 Z 8/16/84 37320 484 Z STO: 18 TEFLON COPOLYMERS 1.0C ; 247 FEP-#2 COAGULATOR - 2ND FLOOR 1/25/84 37924 z462 3/1/84 3792S z451 3/1/84 37926 z451 6/8/84 37927 z464 6/12/84 37928 z465 7/24/84 37929 z456 8/20/84 37930 z470 9/4/84 37931 z481 9/13/84 37932 z466 10/16/34 37033 4 z 12/28/84 37934 z475 BTO ; 18 TEFLON COPOLYMERS LOC: 248 FEP - #1 BLENDER 1/4/84 38151 445 2/1/84 38152 448 3/1/84 38153 3 3/1/84 38154 453 4/3/84 38155 429 4/3/84 38156 429 5/1/84 38157 468 5/1/84 38168 458 5/114 38169 460 6/1/84 38160 460 7/2/84 38161 460 7/00/84 38162 465 s o m 38163 466 8/22/84 38164 469 8/27/84 38166 471 9/4/84 38166 481 z z z z z z z z z z z z z z z z 9/13/84 38167 10/1/84 38168 10/25/84 38169 467 2 z473 z469 Tuesday, January 16,2(301 I t t i 2:03 AM Pers Chemical Cone U nit Percent C-8/FC-143 C-8/FC-143 0.09 MPB 0.03 MPB 16.1% 5.4% C-8/FC-143 CS/FC-143 CS/FC-143 C-8/FC-143 C-8/FC-143 C-8/PC-143 C-8/FC-143 CS/FC-143 C-8/FC-143 CS/FC-143 CS/FC-143 0.74 MPB 0.49 MPB 0.48 MPB 1.32 MPB 1.27 MPB 2.91 MPB OS MPB 1.66 MPB 0.82 MPB 0.31 MPB 0.32 MPB 132.1%" 875% 875% 235.7% " 2265% " 519.6%" 89.3% 296.4% " 146.4% " 55.4% 57.1% C-S/FC-143 . CS/FC-143 C-8/FC-143 C-8/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 CS/FC-143 0.06 MPB 0.08 MPB 0 5 MPB 0,2 MPB 0SB MPB Q2B MPB 0.1 MPB 0,1 MPB 0.35 MPB 0.18 MPB <0.03 MPB 0.19 MPB 0,14 MPB 0.25 MPB 0.29 MPB 0.18 MPB 0.65 MPB 0.09 MPB 0.14 MPB 10.7% 14.3% 35.7% 35.7% 50.0% eo.0% 173% 173% 62.5% 32.1% 5.4% 333% 25.0% 44.6% 51.8% 32.1% 116.1% " 15.1% 25.0% Page 20 o f 23 AJP003944 EID 113079 Sample Dt Samples Duration Type Employee Name 11/12/34 38170 12/6/84 38171 477 Z 469 z BTO: 18 TEFLON COPOLYMERS LOC: 249 FEP-n BLENDER 1/4/84 38049 z447 2/1/84 38050 447 z 3/1/84 38051 3/1/84 38052 4/3/84 38053 453 z z453 429 z 4/3/84 38054 429 2 5/1/84 38055 459 z 5/1/84 38056 459 Z 5/2/84 38057 466 Z S/11/84 38058 6/5/84 38059 460 Z z462 6/12/84 38060 7/5/84 38091 463 z z472 8/3/84 38062 465 z 8/22/84 38063 468 2 9/10/84 38064 466 z 10/12/84 38065 457 z 11/6/84 36066 472 z 12/4/84 38067 475 z BTO: 18 TEFLON COPOLYMERS LOC : 250 B-163 2ND FLOOR LUNCHROOM 12/4/84 37767 468 z BTO: 18 TEFLON COPOLYMERS LOC : 252 2ND FLOOR HALL B-163 2/10/84 37700 453 z BTO: 18 TEFLON COPOLYMERS LOC : 253 B-163 S-W WALL 1ST FLOOR - VEND/MACHS 10/22/84 37988 470 z BTO: 18 LOC : 255 TEFLON COPOLYMERS P/S- FEP EXTRUDER OPERATOR (18PB) 9/12/84 9433 480 p Tuesday, January 16,2001 10:12:03AM Pers Chemical C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 0 8 /F C -1 43 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 none C-8/FC-143 Cone Unit <3,03 MPB 0.1 MPB Percent 5.4% 17.9% 0,23 MPB 0.17 MPB 0.28 MPB 0.28 MPB 0.17 MPB 0.17 MPB 0.13 MPB 0.13 MPB 036 MPB 0.05 MPB 0.15 MPB 028 MPB 0.56 MPB 0.21 MPB 0.12 MPB 0.22 MPB 0.26 MPB <0.03 MPB <0.03 MPB 41.1% 30.4% 50.0% 50.0% 30.4% 30.4% 23,2% 23.2% 64.3% 8.9% 26.8% 50.0% 100.0%** 37.5% 21.4% 39.3% 46.4% 5.4% 5.4% 0.05 MPB 8,9% 0.06 MPB 10.7% 0.07 MPB . .12.5% 0.16 MPB 28.6% Page 21 of 23 AJP003945 EID 113080 Sample Dt Sample# Duration Type Employee Name Pera Chemical BTO: 18 TEFLON COPOLYMERS LOG: 268 FEP-EXTRUDER OPERATOR DESK (CR GONE 9/37) 2/10184 36368 458 2 0/11/84 36369 535 Z C-8/FC-143 C-8/FC-143 BTO: 18 LOG: 269 TEFLON COPOLYMERS PEP - SAMPLING FINISHED PRODUCT BLENDER 4/2/84 39675 5 2 4/2/84 39676 425 2 C-8/FC-143 C-8/FC-143 BTO: 18 TEFLON COPOLYMERS LOG: 273 PEP-FACKOUTROOM-SWCORNER 4/2/84 37794 42D 7 4/2/64 37795 42D Z C-8/FC-143 C-8/FC-143 BTO : 18 LOC; 275 TEFLON COPOLYMERS p/S- FEP PACKOUT ROOM OPERATOR (18PD) 1/31/84 9503 440 P 3/1/84 9904 440 P 5/1/84 9505 460 P 6/12/84 9506 465 P 7/11/64 9507 450 P 7/26/84 9508 462 P 11/7/84 9509 440 P none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 none C-6/FC-143 none C-8/FC-143 none C-B/FC-143 BTO: 18 TEFLON COPOLYMERS LOC: 281 FEP-2ND LEVEL ROOF-HSV FOR FINISHING AREA 1/3/84 34605 444 Z 4/2/84 34606 429 Z BTO : 18 TEFLON COPOLYMERS LOC; 283 BLDG163GENERAL 1/4/84 36730 448 2 1/5/84 36731 440 2 1/6/84 36732 442 Z 1/10/84 36733 445 2 1/10/84 36734 443 Z 1/13/64 36735 452 Z 1/16/84 36736 450 2 1/18/84 36737 449 2 Tuesday, January 16,2001 10:12:03AM C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 Cone Unit Percent <0.03 MPB 016 MPB 5.4% 28.6% <0.03 MPB <0.03 MPB 5.4% 5.4% 0 .0 3 MPB <0.03 MPB 5.4% S.4% 0.1 MPB 0.03 MPB <0.03 MPB 0 0 3 MPB 073 MPB 0 .0 3 MPB 0 0 3 MPB 17.9% 5.4% 5.4% 5.4% 41.1% 5.4% 5.4% 0,14 MPB 0 .0 3 MPB 25.0% 5.4% 0.57 MPB 0.23 MPB 0.43 MPB 0.39 MPB 0.08 MPB 0.33 MPB 0.48 MPB 0.36 MPB 101S % ~ 41.1% 76.8% 69.6% 143% 58.9% 85.7% 64.3% Page22 of23 AJP003946 EID 113081 Sample Dt Sample # Duration Type Employee Name 1/19/84 3673S 1/24/84 36739 2/13/84 36740 3/2/84 36741 3/2/84 36742 5/2/84 36743 6/19/84 36744 7/16/84 36745 8/13/84 36746 9/18/84 36747 10/19/84 36748 11/29/84 36749 12/27/84 36750 463 Z 460 Z 471 Z 447 Z 447 2 432 2 462 Z 364 z 487 z 441 z 468 z 475 z 496 z ' BTO; 18 LOC: 293 TEFLON COPOLYMERS P/S-FEP DISPERSION OPERATOR (18PK) 2/29/84 11799 455 P 6/7/84 11800 465 p 8/6/84 11801 46S p 10/11/84 11802 477 p 12/5/84 11803 465 p Pers Chemical C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-B/FC-143 C-8/PC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C-8/FC-143 C8/FC-143 C-8/FC-143 none C-8/FC-143 none C-S/FC-143 none C-8/FC-143 none C-8/FC-143 none C-8/FC-143 Cone Unit 0.3 MPB 0.37 MPB 038 MPB 0.13 MPB 0.13 MPB 0.14 MPB 0.33 MPB 0.53 MPB 0.21 MPB 0.4 MPB 0.03 MPB 0.05 MPB 0.14 MPB Percent 53.6% 66.1% 67X3% 232% 232% 25.0% 58.9% 946% 37.5% 71.4% 5.4% 89% 25.0% 0.05 MPB <0.03 MPB 0 2 MPB 0.3 MPB 0.43 MPB 89% 5.4% 35.7% 53.6% 76.8% AJP003947 Tuesday, January 16,200110:12:03 AM Page 23 of 23 EID 113082