PHYS* TEST SHEET
jl2R mixed
CURED
TESTED C
LBS, Tbs. LBS. LBS.
f%%
% BREAK
TENS. TENS. TENS. TENS, TENS.
'HARD
% * f* BREAK ELONG NESS SET
3\i 730 in
[300 3QO
300 TOO 300 300
KbS
j
|. . 08k 1 mi
3, , 08 b
0
<r/f 7 l(o 315 on 9 \3
'2S$> 35o ?5c,2 IpQ
7 by? TVFo
CHARDO 00042
C.
-O--nJFp
ressi
OM?] "O y
e\ 1
Z
d
rmr
----- .. To Tt
.379 TbT ,503 SOT
4-OZ
4cb
6*711 o -Tt
otT ,|0\ oOT
31b 37 5 obp
378
315
To Tb
,107 1 2,8 T?p
%5e3 71-0 033 789 734
ji\w
IVve
73 V)
7S
'N 0,1
'
ZF
.1 - CRL
Z. . (. BZ
3 090 .
\ J CjHh
..
o73>.,11
093
03T
T5T1 73 T
; ----- 1--1yo ,
1
300 2SO 300 7^0 3C0 130 L. b 1 1Z2S 303 I IZco IZ1S S |3od>! 3bo
S
' ----- 1
#
Rubber Division
373 Washington Street, Chardon, Ohio 44024 (216) 285-2161
CERTIFICATION OF TEST RESULTS
Date: For: Whirlpool
Order No.: Part No.: (g^SKoZ
Attention:
Mat^l. Spec. Compound No.: VWoO I
ORIGINAL UNAGED PROPERTIES Tensile strength~Ps-i Elongation, $ Durometer Color
AIR OVEN AGED "7 Q HRS . @
tensile Strength, rJT~change Elongation, % Change Durometer, Change
F
- COMPRESSION^T METHOD B 21 HRS.,
REQUIRED
OBTAINED
Pcxss V \ 3 Po.SS PZy'PGjZS
These test results are certified to he accurate and representative of the submitted samples as determined by tests conducted by our laboratory. CHARDON RUBBER COMPANY
I
CHARDO 00043
Rubber division
373 Washington Street, Chardon, Ohio 44024 (215.1 285-2161
CERTIFICATION OF TEST RESULTS
Date ,* A*V"7 -80
Order No.:
For: VlVnripOol
Part No.: m^KoT.
Attention:
Mat 1. Spec.:
-
Compound No.: V -^sOO
ORIGINAL UWAGED PROPERTIES TertsTle " StFength7_p'si Elongation, $ Durometer Color
AIR OVEN AGED "?Q HRS. 7.Q. F
Tensile Strength,"'% Change Elongation, % Change Durometer, Change
REQUIRED
Zgseri
ziSrnz
COMPRESSION SET METHOD B *IX HRS. @'KZF
FSeS--------------------- ------------------------ -
Ci j
^
901 Phx*
P I > Po.s-5 ^
OBTAINED
32
.SAodfe..
j-J
2 "i ^ (t-t
No Chflunotf .tlfepeiwfe
-4 i "i* .i/i 2 #
&7.S1
7^ /
cv
These test results are certified to be accurate and representative of the submitted samples as determined by tests conducted by our laboratory. CHARDON RUBBER COMPANY
CHARDO 00044
373 Wosktngion Streel Chpidon, Ohio 44024 (216)2B5'2W
certification of test results
Date: 7*2.1-81 For: Whirlpool Attention:
Order No.:
Part No.: (D8'ET7<bP.
Mat'l. Spec.:BK<bOAB\V(BO%^M^ Cijp\yp2.
Compound No.: V-<oOO\
ORIGINAL UNAGED PROPERTIES Tensile Strength, psi Elongation, % Durometer Color
AIR OVEN AGED IQ
HRS. 0 Z]2. J_
Tensile Strength, % Change
Elongation, % Change
Durometer, Change
#
COMPRESSION SET METHOD B 2,2. % Set
HRS. @ 2R.F
REQUIRED
OBTAINED
t*5cf70
-vPC?*
i \SpnvAs. + 4-points
8Q7oW 72.5%
Ci^ Rx_SS v \; pass P2j Pass
These test results are certified to be accurate and representative of the.submitted samples as determined by tests conducted by our laboratory.
CHARDON RUBBER COMPANY
Richard F. Znidarsic Chief Chemist
RFZ/dk
f
CHARDO 00045
373 Wbshington Street Chordon. Ohio 44024 (2/6)285 2)6)
CERTIFICATION QF TEST RESULTS
Date: 7-21-81
For: W V\ir IpOol
Attention:
Order No.: Part No.: CdQ'oT<0*2. Mafl. Spec.:BK(bOA-'b\4CBO<7oMKX) Compound No.: V-<bOO\
ORIGINAL UNAGED PROPERTIES Tensile Strength, psi
Elongation, %
Durometer Color
AIR OVEN AGED ~7Q
HRS, @2.l2.QF
Tensile Strength, Change Elongation, Change Durometer, Change
COMPRE S SI ON SET METHOD B 2.2. % Set
HRS. P 2R.F
REQUIRED 4-00
OBTAINED S2.S
W1
'feAojc.k
t'SCtt,
+207. + 4-po\rAs
72.S7.
C\ y Rx.ss
P \ i Pass
P^jPass
These test results are certified to be accurate and representative of the submitted samples as determined by tests conducted by our laboratory. CHARDON RUBBER COMPANY
Richard F. Znidarsic Chief Chemist RFZ/dk
CHARDO 00046
\
* Cbardon Rubber
Company
373 Wnhmgton Street Chonkm, Ohio *4034 (316)285-3161
Date:
14*^81
For: Nor^e.
Attention: b
>
CERTIFICATION OF TEST RESULTS Order No.:
3>
^PluGS
Le^-V Lab
part No.:
Hafl. Spec :
VfcO .Compound No.:
02
TPR frem CKni -tO.OS doAe
ORISIHAl UNA6ED PROPERTIES Tensile Strength, psi
Elongation, % Durometer Color rl-
70AIR OVEN AGED
HRS. 0 2XL'f
Tensile Strength, % Change
Elongation, % Change
Durometer, Change
COMPRESSION SET METHOD B ti- HRS, e Zft.F * Set
REQUIRED
OBTAINED
80pw JOS.
cii ^ss
Pi i Thas
Wi Pass
These test results are certified to be accurate and representative of the.submitted samples as determined' by tests conducted by our laboratory. CKARDON RUBBER COMPANY
Richard F. Znldarsic Chief Chemist RFZ/dk
CHARDO 00047
Industrial Rubber Goods Division
1776 Hilltop Road
St. Joseph, Michigan 49085 (616)933-7741
Dick Zandarstc CHARDON RUBBER COMPANY 373 Washington St. Chardon, Ohio 44024
Dear Dick:
SUBJECT: Slabs & Buttons from TPR (Grey color requested}.
Norge, Purchasing, and Engineering are most Interested In*the possibility of using TPR. as a replacement for thetr current dryer door gasket material. Please prepare slabs & buttons along with certification and foward same to my attention. I flope this can be done within the next few weeks as the cost savings to Norge Is of great Importance. In addition competition Is working
to take the current business from us with lower prices.
4
Please advise your date which you can provide slabs & buttons.
Cordially,
c.c. Chris Terry ASD/js
A. S. Dloehy Marketing/ Manager
CHARDO 00048
jr/2 '-y.it
Ct J'oon 0" *4374
rjit)7Sb ?I6I
CERTIFICATION QF TEST RESULTS
Date:
April 13, 1981
For:
Norge on;
Order Ho.: Part No.:
Mat']. Spec.: BA604M4(80% Max.)ciPlP2
Compound No.: V-6001
0 I h l \ A I. U NA G ED _ PROPERTIES iV:sile Strength, psi
jlion-, %
D.,r ter
Color
air oven aged 70
hrs.
T+isile Strength, % C! anje
[lufget7on, t Change
Puro.Tieter, Change
p__2.12_
CCrrRtSSION _StT_MET.-`OD S' 22
% Sot
HRS. P 212 _F
REQ_U_I_RED
A0_O__ _ 250 ,,6Q/" 5_ Black
OBTAINED
n;>p..... .. 235 ....64___ _ Black
Ui1o i
+/-30Z +/-15
+14.0
-21.2 4-2
80 max.
70.6
Cl: Pass
These test results are certified to be accurate and representative of the. submitted samples as determined by tests conducted by our laboratory.
CHARDON RUBBER COMPANY
Richard F. Znidarsic Chief Chemist
RfZ/dk
CHARDO 00049